EN 573-3 Grade AW-8079 H19

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlFeSi alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,Aludium,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H19

EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3

Foil

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H19

EN 573-3, EN 683

Foil

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.06 mm

Show Material materials with Thickness of 0.06 mm

H19

EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3

0.06 mm

Foil

1.00 mm

Show Material materials with Thickness of 1.00 mm

H19

EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3

1.00 mm

Foil

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

69.0 - 72.0 GPa

Show Material materials with Elastic modulus of 69.0 - 72.0 GPa

Typical for Wrought 8000 Series Aluminium

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 8000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 8000 Series Aluminium

Tensile strength

170.0 - 175.0 MPa

Show Material materials with Tensile strength of 170.0 - 175.0 MPa

H19

EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3

Foil

170.0 MPa

Show Material materials with Tensile strength of 170.0 MPa

H19

EN 573-3, EN 683

Foil

20.0 °C

170.0 MPa

Show Material materials with Tensile strength of 170.0 MPa

H19

EN 573-3

Foil

20.0 °C

175.0 MPa

Show Material materials with Tensile strength of 175.0 MPa

H19

EN 573-3

Foil

Yield strength

155.0 MPa

Show Material materials with Yield strength of 155.0 MPa

H19

EN 573-3, EN 683

Foil

RP02

155 MPa

Show Material materials with Yield strength of 155 MPa

H19

EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3

Foil

20.0 °C

155.0 MPa

Show Material materials with Yield strength of 155.0 MPa

H19

EN 573-3

Foil

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H19

EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3

Foil

Melting point

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

Typical for Wrought 8000 Series Aluminium

Specific heat capacity

920.0 J/(kg·K)

Show Material materials with Specific heat capacity of 920.0 J/(kg·K)

Typical for Wrought 8000 Series Aluminium

Thermal conductivity

167.0 - 220.0 W/(m·K)

Show Material materials with Thermal conductivity of 167.0 - 220.0 W/(m·K)

Typical for Wrought 8000 Series Aluminium

Electrical

PropertyValueComment

Electrical conductivity

28000000.0 - 35000000.0 S/m

Show Material materials with Electrical conductivity of 28000000.0 - 35000000.0 S/m

Typical for Wrought 8000 Series Aluminium

Electrical resistivity

2.8e-08 - 3.5e-08 Ω·m

Show Material materials with Electrical resistivity of 2.8e-08 - 3.5e-08 Ω·m

Typical for Wrought 8000 Series Aluminium

Chemical properties

PropertyValueConditionRelated StandardsShape

Copper

0.05 %

Show Material materials with Copper of 0.05 %

H19

EN 573-3, EN 683

Foil

0.05 %

Show Material materials with Copper of 0.05 %

H19

EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3

Foil

Iron

0.7 - 1.3 %

Show Material materials with Iron of 0.7 - 1.3 %

H19

EN 573-3, EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 683

Foil

Silicon

0.05 - 0.3 %

Show Material materials with Silicon of 0.05 - 0.3 %

H19

EN 573-3, EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3, EN 683

Foil

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H19

EN 573-3, EN 683

Foil

0.1 %

Show Material materials with Zinc of 0.1 %

H19

EN 546-2, EN 683-2, EN 573-1, EN 573-2, EN 573-3

Foil

Technological properties

Property
Application areas

Roofing: Foil for bituminous coating; Heat exchangers: Fins, Heat exchangers; Insulation; Semi-rigid and corrugated: Pet food; Foil stock: Foil app; Components: Automotive fins, Heat exchangers

Corrosion properties

Moderated

Workability

Excellent