EN 573-3 Grade AW-3003 H14

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-3003 is a popular alloy that offers customers very good atmospheric corrosion resistance and moderate strength. Aluminum 3003 offers good machinability for aluminum alloys, though it is not heat treatable. Unlike other aluminum alloys, EN AW-3003 is weldable by conventional welding methods. It also takes cold and hot working well and has generally better mechanical properties when compared to 1000 series aluminum alloys.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

65.0 MPa

Show Material materials with Bending Fatigue Strength of 65.0 MPa

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Bending angle 180°

2.0 °/t

Show Material materials with Bending angle 180° of 2.0 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

60.0 - 70.0 GPa

Show Material materials with Elastic modulus of 60.0 - 70.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

60.0 - 65.0 GPa

Show Material materials with Elastic modulus of 60.0 - 65.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

60.0 - 69.5 GPa

Show Material materials with Elastic modulus of 60.0 - 69.5 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

60.0 - 69.0 GPa

Show Material materials with Elastic modulus of 60.0 - 69.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

65.0 - 70.0 GPa

Show Material materials with Elastic modulus of 65.0 - 70.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

65.0 - 69.5 GPa

Show Material materials with Elastic modulus of 65.0 - 69.5 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

65.0 - 69.0 GPa

Show Material materials with Elastic modulus of 65.0 - 69.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

69.0 - 70.0 GPa

Show Material materials with Elastic modulus of 69.0 - 70.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

69.0 - 69.5 GPa

Show Material materials with Elastic modulus of 69.0 - 69.5 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

69.5 - 70.0 GPa

Show Material materials with Elastic modulus of 69.5 - 70.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3, EN 485, EN 541

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A100

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

A100

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3

Foil

A50

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3

Foil

A100

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3

Sheet, Flat

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3

Flat

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3

Rod, Tube, Flat

A50

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Flat

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Sheet

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Flat

Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H14

EN 573-3

Wire

A100

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3

Sheet

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H14

EN 573-3

Rod, Tube

Hardness, Brinell

46.0 [-]

Show Material materials with Hardness, Brinell of 46.0 [-]

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

40.0 [-]

Show Material materials with Hardness, Brinell of 40.0 [-]

H14

EN 573-3

Rod, Tube

20.0 °C

46.0 [-]

Show Material materials with Hardness, Brinell of 46.0 [-]

H14

EN 573-3

Flat, Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

24.0 - 26.5 GPa

Show Material materials with Shear modulus of 24.0 - 26.5 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

24.0 - 26.1 GPa

Show Material materials with Shear modulus of 24.0 - 26.1 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

26.1 - 26.5 GPa

Show Material materials with Shear modulus of 26.1 - 26.5 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

Tensile strength

20.0 °C

120.0 - 185.0 MPa

Show Material materials with Tensile strength of 120.0 - 185.0 MPa

H14

EN 573-3

Sheet

20.0 °C

120.0 - 160.0 MPa

Show Material materials with Tensile strength of 120.0 - 160.0 MPa

H14

EN 573-3

Sheet

20.0 °C

130.0 - 165.0 MPa

Show Material materials with Tensile strength of 130.0 - 165.0 MPa

H14

EN 573-3, EN 754

Rod, Tube, Strip, Sheet, Plate, Foil, Wire, Bar

20.0 °C

135.0 - 180.0 MPa

Show Material materials with Tensile strength of 135.0 - 180.0 MPa

H14

EN 573-3, EN 1301

Wire, Strip, Sheet, Plate, Foil, Tube, Bar

20.0 °C

140.0 - 180.0 MPa

Show Material materials with Tensile strength of 140.0 - 180.0 MPa

H14

EN 573-3

Foil

20.0 °C

145.0 - 185.0 MPa

Show Material materials with Tensile strength of 145.0 - 185.0 MPa

H14

EN 573-3, EN 485, EN 541, EN 683

Foil, Sheet, Flat, Strip, Plate, Wire, Tube, Bar

20.0 °C

145.0 - 160.0 MPa

Show Material materials with Tensile strength of 145.0 - 160.0 MPa

H14

EN 573-3

Sheet

20.0 °C

145.0 - 185.0 MPa

Show Material materials with Tensile strength of 145.0 - 185.0 MPa

H14

EN 573-3

Flat

Transverse

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

-50 °C

2.1499999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

-50.0 °C

2.15e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.15e-05 1/K

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20 °C

2.1499999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

20 °C

2.52e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

100.0 °C

2.32e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.32e-05 1/K

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

200 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

200.0 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

300 °C

2.52e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

300.0 °C

2.52e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

Melting point

640.0 - 655.0 °C

Show Material materials with Melting point of 640.0 - 655.0 °C

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

643.0 - 654.0 °C

Show Material materials with Melting point of 643.0 - 654.0 °C

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Specific heat capacity

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

892.0 - 893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 892.0 - 893.0 J/(kg·K)

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

892.0 J/(kg·K)

Show Material materials with Specific heat capacity of 892.0 J/(kg·K)

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

Thermal conductivity

159.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 159.0 - 193.0 W/(m·K)

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

160.0 - 200.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 200.0 W/(m·K)

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

20.0 °C

160.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 W/(m·K)

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

24000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 24000000.0 - 29000000.0 S/m

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

22000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 22000000.0 - 29000000.0 S/m

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

23000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 29000000.0 S/m

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar, Rod, Flat

Electrical resistivity

3.45e-08 - 4.17e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 4.17e-08 Ω·m

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

3.45e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 4.35e-08 Ω·m

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

20.0 °C

3.4e-08 - 4.1e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 4.1e-08 Ω·m

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

3.4e-08 - 4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 4.5e-08 Ω·m

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

4.1e-08 Ω·m

Show Material materials with Electrical resistivity of 4.1e-08 Ω·m

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

20.0 °C

4.1e-08 - 4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.1e-08 - 4.5e-08 Ω·m

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Copper

0.05 - 0.2 %

Show Material materials with Copper of 0.05 - 0.2 %

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Rod, Sheet, Flat, Foil, Tube, Wire, Strip, Plate, Bar

Iron

0.7 %

Show Material materials with Iron of 0.7 %

H14

EN 573-3

Rod, Sheet, Flat, Foil, Tube, Wire

0.70 %

Show Material materials with Iron of 0.70 %

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Strip, Sheet, Plate, Foil, Wire, Tube, Bar

Manganese

1.0 - 1.5 %

Show Material materials with Manganese of 1.0 - 1.5 %

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Rod, Sheet, Flat, Foil, Tube, Wire, Strip, Plate, Bar

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Rod, Sheet, Flat, Foil, Tube, Wire, Strip, Plate, Bar

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H14

EN 573-3, EN 1301, EN 485, EN 541, EN 683, EN 754

Rod, Sheet, Flat, Foil, Tube, Wire, Strip, Plate, Bar

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Brazing

hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: good, weathering: very good

Workability