EN 573-3 Grade AW-3004 O

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMn alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

20.0 °C

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Flat, Sheet, Strip

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

0.2 mm

Sheet, Strip

2 mm

Show Material materials with Thickness of 2 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

2 mm

Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

0 °/t

Show Material materials with Bending angle 180° of 0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

Bending angle 90°

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

Elastic modulus

68.6 GPa

Show Material materials with Elastic modulus of 68.6 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

Elongation

-196.0 °C

38.0 %

Show Material materials with Elongation of 38.0 %

O

EN 573-3

-80.0 °C

30.0 %

Show Material materials with Elongation of 30.0 %

O

EN 573-3

-28.0 °C

26.0 %

Show Material materials with Elongation of 26.0 %

O

EN 573-3

1 %

Show Material materials with Elongation of 1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

A50

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

A50

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

A50

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

A100

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

A50

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

A50

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

O

EN 573-3

Flat

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3

Flat

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3

Flat

Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

O

EN 573-3

Flat

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Flat

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3

Flat

A50

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

O

EN 573-3

100.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

O

EN 573-3

150.0 °C

35.0 %

Show Material materials with Elongation of 35.0 %

O

EN 573-3

200.0 °C

55.0 %

Show Material materials with Elongation of 55.0 %

O

EN 573-3

260.0 °C

70.0 %

Show Material materials with Elongation of 70.0 %

O

EN 573-3

315.0 °C

80.0 %

Show Material materials with Elongation of 80.0 %

O

EN 573-3

370.0 °C

90.0 %

Show Material materials with Elongation of 90.0 %

O

EN 573-3

Hardness, Brinell

45.0 [-]

Show Material materials with Hardness, Brinell of 45.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

20.0 °C

45.0 [-]

Show Material materials with Hardness, Brinell of 45.0 [-]

O

EN 573-3

Flat

Hardness, HBW

45.0 - 80.0 [-]

Show Material materials with Hardness, HBW of 45.0 - 80.0 [-]

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Shear modulus

26.0 GPa

Show Material materials with Shear modulus of 26.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

20.0 °C

25.0 - 27.0 GPa

Show Material materials with Shear modulus of 25.0 - 27.0 GPa

O

EN 573-3

Flat

Tensile strength

-196.0 °C

290.0 MPa

Show Material materials with Tensile strength of 290.0 MPa

O

EN 573-3

-80.0 °C

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

O

EN 573-3

-28.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

O

EN 573-3

155.0 - 330.0 MPa

Show Material materials with Tensile strength of 155.0 - 330.0 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

20.0 °C

155.0 - 200.0 MPa

Show Material materials with Tensile strength of 155.0 - 200.0 MPa

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube, Flat

20.0 °C

155.0 - 200.0 MPa

Show Material materials with Tensile strength of 155.0 - 200.0 MPa

O

EN 573-3

Flat

Transverse

20.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

O

EN 573-3

100.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

O

EN 573-3

150.0 °C

150.0 MPa

Show Material materials with Tensile strength of 150.0 MPa

O

EN 573-3

200.0 °C

95.0 MPa

Show Material materials with Tensile strength of 95.0 MPa

O

EN 573-3

260.0 °C

70.0 MPa

Show Material materials with Tensile strength of 70.0 MPa

O

EN 573-3

315.0 °C

50.0 MPa

Show Material materials with Tensile strength of 50.0 MPa

O

EN 573-3

370.0 °C

35.0 MPa

Show Material materials with Tensile strength of 35.0 MPa

O

EN 573-3

Yield strength

-196.0 °C

90.0 MPa

Show Material materials with Yield strength of 90.0 MPa

O

EN 573-3

RP02

-80.0 °C

75.0 MPa

Show Material materials with Yield strength of 75.0 MPa

O

EN 573-3

RP02

-28.0 °C

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

O

EN 573-3

RP02

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

RP02

60.0 - 310.0 MPa

Show Material materials with Yield strength of 60.0 - 310.0 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

20.0 °C

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3

Flat

RP02

20.0 °C

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3

Flat

RP02 Transverse

20.0 °C

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

O

EN 573-3

RP02

100.0 °C

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

O

EN 573-3

RP02

150.0 °C

70.0 MPa

Show Material materials with Yield strength of 70.0 MPa

O

EN 573-3

RP02

200.0 °C

65.0 MPa

Show Material materials with Yield strength of 65.0 MPa

O

EN 573-3

RP02

260.0 °C

50.0 MPa

Show Material materials with Yield strength of 50.0 MPa

O

EN 573-3

RP02

315.0 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

RP02

370.0 °C

20.0 MPa

Show Material materials with Yield strength of 20.0 MPa

O

EN 573-3

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

-50 °C

2.1499999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

-50.0 °C

2.15e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.15e-05 1/K

O

EN 573-3

Flat

20 °C

2.1499999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

20 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

20 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube, Flat

20 °C

2.51e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube, Flat

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

100.0 °C

2.32e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.32e-05 1/K

O

EN 573-3

Flat

100 °C

2.3899999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

20-100°C

200 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube, Flat

200.0 °C

2.41e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube, Flat

300 °C

2.51e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube, Flat

300.0 °C

2.51e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube, Flat

Melting point

629.0 - 654.0 °C

Show Material materials with Melting point of 629.0 - 654.0 °C

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

630.0 - 655.0 °C

Show Material materials with Melting point of 630.0 - 655.0 °C

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

Specific heat capacity

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

20.0 °C

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

O

EN 573-3

Flat

Thermal conductivity

160.0 - 180.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 180.0 W/(m·K)

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

163 W/(m·K)

Show Material materials with Thermal conductivity of 163 W/(m·K)

O

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Strip, Sheet, Plate, Foil, Welded Tube, Strip

20.0 °C

160.0 - 190.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 190.0 W/(m·K)

O

EN 573-3

Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

23000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 25000000.0 S/m

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

24000000.0 S/m

Show Material materials with Electrical conductivity of 24000000.0 S/m

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

20.0 °C

20000000.0 - 24000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 24000000.0 S/m

O

EN 573-3

Flat

Electrical resistivity

4e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 4e-08 - 4.35e-08 Ω·m

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

4.0999999999999997e-08 Ω·m

Show Material materials with Electrical resistivity of 4.0999999999999997e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

4.17e-08 Ω·m

Show Material materials with Electrical resistivity of 4.17e-08 Ω·m

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Copper

0.25 %

Show Material materials with Copper of 0.25 %

O

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Foil, Welded Tube

0.25 %

Show Material materials with Copper of 0.25 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

Iron

0.7 %

Show Material materials with Iron of 0.7 %

O

EN 573-3

Flat

0.70 %

Show Material materials with Iron of 0.70 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Welded Tube

0.7 %

Show Material materials with Iron of 0.7 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

Magnesium

0.8 - 1.3 %

Show Material materials with Magnesium of 0.8 - 1.3 %

O

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Flat, Strip, Sheet, Plate, Foil, Welded Tube, Strip

Manganese

1.0 - 1.5 %

Show Material materials with Manganese of 1.0 - 1.5 %

O

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Flat, Strip, Sheet, Plate, Foil, Welded Tube, Strip

Silicon

0.3 %

Show Material materials with Silicon of 0.3 %

O

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Foil, Welded Tube

0.3 %

Show Material materials with Silicon of 0.3 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

O

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Foil, Welded Tube

0.25 %

Show Material materials with Zinc of 0.25 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541

Sheet, Strip

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Intermediate transformation/interior use; Heat exchangers: Fins; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Food can: Body, Lids; Semi-rigid and corrugated: Smooth wall

Brazing

Very Good

Corrosion properties

Seawater: very good, weathering: very good

Welding

Very Good

Workability

Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12)