EN 573-3 Grade AW-3005 H14

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMn alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H14

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Welded Tube

20.0 °C

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H14

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Flat, Seamless Tube, Coil, Sheet

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.3 mm

Show Material materials with Thickness of 0.3 mm

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

0.3 mm

Coil, Sheet

1.5 mm

Show Material materials with Thickness of 1.5 mm

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

1.5 mm

Coil, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

1.5 °/t

Show Material materials with Bending angle 180° of 1.5 °/t

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

2.5 °/t

Show Material materials with Bending angle 180° of 2.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

2.0 °/t

Show Material materials with Bending angle 90° of 2.0 °/t

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H14

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Welded Tube

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

A50

1 %

Show Material materials with Elongation of 1 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

A50

7.0 %

Show Material materials with Elongation of 7.0 %

H14

EN 573-3, EN 1592

Strip, Sheet, Plate, Welded Tube

A100

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H14

EN 573-3

Flat

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H14

EN 573-3

Flat

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3

Flat

A50 Transverse

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H14

EN 573-3

Flat

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H14

EN 573-3

Seamless Tube

Hardness, Brinell

54.0 [-]

Show Material materials with Hardness, Brinell of 54.0 [-]

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

20.0 °C

54.0 [-]

Show Material materials with Hardness, Brinell of 54.0 [-]

H14

EN 573-3

Flat

Hardness, HBW

53 [-]

Show Material materials with Hardness, HBW of 53 [-]

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Shear modulus

26.0 GPa

Show Material materials with Shear modulus of 26.0 GPa

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

20.0 °C

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H14

EN 573-3

Flat, Seamless Tube

Tensile strength

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H14

EN 573-3, EN 1592

Strip, Sheet, Plate, Welded Tube

20.0 °C

170.0 - 215.0 MPa

Show Material materials with Tensile strength of 170.0 - 215.0 MPa

H14

EN 573-3

Flat

Transverse

20.0 °C

170.0 - 215.0 MPa

Show Material materials with Tensile strength of 170.0 - 215.0 MPa

H14

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Flat, Strip, Sheet, Plate, Welded Tube, Coil, Sheet

20.0 °C

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H14

EN 573-3

Seamless Tube

Yield strength

130 MPa

Show Material materials with Yield strength of 130 MPa

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

150.0 MPa

Show Material materials with Yield strength of 150.0 MPa

H14

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

RP02

175.0 MPa

Show Material materials with Yield strength of 175.0 MPa

H14

EN 573-3, EN 1592

Strip, Sheet, Plate, Welded Tube

RP02

20.0 °C

150.0 MPa

Show Material materials with Yield strength of 150.0 MPa

H14

EN 573-3

Flat

RP02 Transverse

20.0 °C

150.0 MPa

Show Material materials with Yield strength of 150.0 MPa

H14

EN 573-3

Flat

RP02

20.0 °C

175.0 MPa

Show Material materials with Yield strength of 175.0 MPa

H14

EN 573-3

Seamless Tube

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Welded Tube

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H14

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Welded Tube

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

20-100°C

Melting point

630.0 - 654.0 °C

Show Material materials with Melting point of 630.0 - 654.0 °C

H14

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Welded Tube

Specific heat capacity

20.0 °C

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H14

EN 573-3

Flat, Seamless Tube

Thermal conductivity

160.0 - 190.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 190.0 W/(m·K)

H14

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Welded Tube

172 W/(m·K)

Show Material materials with Thermal conductivity of 172 W/(m·K)

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

20.0 °C

200.0 W/(m·K)

Show Material materials with Thermal conductivity of 200.0 W/(m·K)

H14

EN 573-3

Flat, Seamless Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

23000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 25000000.0 S/m

H14

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Welded Tube

20.0 °C

28000000.0 S/m

Show Material materials with Electrical conductivity of 28000000.0 S/m

H14

EN 573-3

Flat, Seamless Tube

Electrical resistivity

3.7999999999999996e-08 Ω·m

Show Material materials with Electrical resistivity of 3.7999999999999996e-08 Ω·m

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

4e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 4e-08 - 4.35e-08 Ω·m

H14

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Welded Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H14

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube

0.1 %

Show Material materials with Chromium of 0.1 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

Copper

0.3 %

Show Material materials with Copper of 0.3 %

H14

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube

0.3 %

Show Material materials with Copper of 0.3 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

Iron

0.7 %

Show Material materials with Iron of 0.7 %

H14

EN 573-3

Flat, Seamless Tube

0.70 %

Show Material materials with Iron of 0.70 %

H14

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Welded Tube

0.7 %

Show Material materials with Iron of 0.7 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

Magnesium

0.2 - 0.6 %

Show Material materials with Magnesium of 0.2 - 0.6 %

H14

EN 573-3, EN 1592, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube, Coil, Sheet

Manganese

1.0 - 1.5 %

Show Material materials with Manganese of 1.0 - 1.5 %

H14

EN 573-3, EN 1592, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube, Coil, Sheet

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

H14

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube

0.6 %

Show Material materials with Silicon of 0.6 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

H14

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H14

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Welded Tube

0.25 %

Show Material materials with Zinc of 0.25 %

H14

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541

Coil, Sheet

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Electronic devices: Housing of devices; Insulation; Cosmetics: Cosmetics pieces

Brazing

Good

Corrosion properties

Seawater: very good, weathering: very good

Welding

Good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / acceptable (H12)