EN 573-3 Grade AW-3005 H12

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMn alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

20.0 °C

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

H12

EN 573-3

Flat

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

1.5 °/t

Show Material materials with Bending angle 180° of 1.5 °/t

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

2.0 °/t

Show Material materials with Bending angle 180° of 2.0 °/t

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

Bending angle 90°

0.5 °/t

Show Material materials with Bending angle 90° of 0.5 °/t

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

Hardness, Brinell

46.0 [-]

Show Material materials with Hardness, Brinell of 46.0 [-]

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

20.0 °C

46.0 [-]

Show Material materials with Hardness, Brinell of 46.0 [-]

H12

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Shear modulus

20.0 °C

26.5

Show Material materials with Shear modulus of 26.5

H12

EN 573-3

Flat

Tensile strength

20.0 °C

145.0 - 195.0 MPa

Show Material materials with Tensile strength of 145.0 - 195.0 MPa

H12

EN 573-3

Flat

Transverse

20.0 °C

145.0 - 195.0 MPa

Show Material materials with Tensile strength of 145.0 - 195.0 MPa

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube, Flat

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

Melting point

630.0 - 654.0 °C

Show Material materials with Melting point of 630.0 - 654.0 °C

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

Specific heat capacity

20.0 °C

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

H12

EN 573-3

Flat

Thermal conductivity

160.0 - 190.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 190.0 W/(m·K)

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

20.0 °C

200.0 W/(m·K)

Show Material materials with Thermal conductivity of 200.0 W/(m·K)

H12

EN 573-3

Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

23000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 25000000.0 S/m

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

20.0 °C

28000000.0 S/m

Show Material materials with Electrical conductivity of 28000000.0 S/m

H12

EN 573-3

Flat

Electrical resistivity

4e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 4e-08 - 4.35e-08 Ω·m

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Welded Tube

Copper

0.3 %

Show Material materials with Copper of 0.3 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Welded Tube

Iron

0.7 %

Show Material materials with Iron of 0.7 %

H12

EN 573-3

Flat

0.70 %

Show Material materials with Iron of 0.70 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Welded Tube

Magnesium

0.2 - 0.6 %

Show Material materials with Magnesium of 0.2 - 0.6 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Welded Tube

Manganese

1.0 - 1.5 %

Show Material materials with Manganese of 1.0 - 1.5 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Welded Tube

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Welded Tube

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Welded Tube

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H12

EN 573-3, EN 485

Flat, Strip, Sheet, Plate, Welded Tube

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (O) / acceptable (H12)