EN 573-3 Grade AW-3103 O

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMn alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Foil, Rod, Sheet, Flat, Tube, Wire, Coil, Sheet

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.035 mm

Show Material materials with Thickness of 0.035 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.035 mm

Coil, Sheet

4.0 mm

Show Material materials with Thickness of 4.0 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

4.0 mm

Coil, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

50.0 MPa

Show Material materials with Bending Fatigue Strength of 50.0 MPa

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 180°

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Bending angle 90°

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Elastic modulus

-270 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire, Coil, Sheet

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire, Coil, Sheet

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

69.0 - 70.0 GPa

Show Material materials with Elastic modulus of 69.0 - 70.0 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

69.0 - 69.5 GPa

Show Material materials with Elastic modulus of 69.0 - 69.5 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

20.0 °C

69.5 - 70.0 GPa

Show Material materials with Elastic modulus of 69.5 - 70.0 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire, Coil, Sheet

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire, Coil, Sheet

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

300 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

Elongation

-196.0 °C

46.0 %

Show Material materials with Elongation of 46.0 %

O

EN 573-3

-80.0 °C

42.0 %

Show Material materials with Elongation of 42.0 %

O

EN 573-3

-20.0 °C

41.0 %

Show Material materials with Elongation of 41.0 %

O

EN 573-3

7.0 %

Show Material materials with Elongation of 7.0 %

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

8.0 %

Show Material materials with Elongation of 8.0 %

O

EN 573-3, EN 546

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

17.0 %

Show Material materials with Elongation of 17.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

17.0 - 21.0 %

Show Material materials with Elongation of 17.0 - 21.0 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

A50

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

21.0 %

Show Material materials with Elongation of 21.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

25.0 %

Show Material materials with Elongation of 25.0 %

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A100

28.0 %

Show Material materials with Elongation of 28.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

A50

35.0 %

Show Material materials with Elongation of 35.0 %

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

O

EN 573-3

Foil

A100

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

O

EN 573-3

Foil

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

O

EN 573-3

Foil

A100

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

O

EN 573-3

Foil

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3

Foil

A100

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3

Foil

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Foil

A100

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Foil

A50

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

O

EN 573-3

Flat

A50

20.0 °C

17.0 %

Show Material materials with Elongation of 17.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Foil

A100

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Foil, Sheet

A50

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3

Flat

A50

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Rod, Tube

A50

20.0 °C

21.0 %

Show Material materials with Elongation of 21.0 %

O

EN 573-3

Flat

A50

20.0 °C

21.0 %

Show Material materials with Elongation of 21.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3

Tube

20.0 °C

23.0 %

Show Material materials with Elongation of 23.0 %

O

EN 573-3

Sheet

A50

20.0 °C

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3

Flat

A50

20.0 °C

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

O

EN 573-3

Rod, Tube, Flat

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

O

EN 573-3

Flat

Transverse

20.0 °C

28.0 %

Show Material materials with Elongation of 28.0 %

O

EN 573-3

Flat

A50

20.0 °C

28.0 %

Show Material materials with Elongation of 28.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

35.0 %

Show Material materials with Elongation of 35.0 %

O

EN 573-3

Wire

A100

20.0 °C

40.0 %

Show Material materials with Elongation of 40.0 %

O

EN 573-3

100.0 °C

43.0 %

Show Material materials with Elongation of 43.0 %

O

EN 573-3

150.0 °C

47.0 %

Show Material materials with Elongation of 47.0 %

O

EN 573-3

200.0 °C

60.0 %

Show Material materials with Elongation of 60.0 %

O

EN 573-3

260.0 °C

65.0 %

Show Material materials with Elongation of 65.0 %

O

EN 573-3

320.0 °C

70.0 %

Show Material materials with Elongation of 70.0 %

O

EN 573-3

370.0 °C

70.0 %

Show Material materials with Elongation of 70.0 %

O

EN 573-3

Hardness, Brinell

27.0 [-]

Show Material materials with Hardness, Brinell of 27.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

27.0 [-]

Show Material materials with Hardness, Brinell of 27.0 [-]

O

EN 573-3

Flat

20.0 °C

28.0 [-]

Show Material materials with Hardness, Brinell of 28.0 [-]

O

EN 573-3

Rod, Tube

20.0 °C

29.0 [-]

Show Material materials with Hardness, Brinell of 29.0 [-]

O

EN 573-3

Rod, Tube

Hardness, HBW

27 [-]

Show Material materials with Hardness, HBW of 27 [-]

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

24.0 - 26.5 GPa

Show Material materials with Shear modulus of 24.0 - 26.5 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

24.0 - 26.1 GPa

Show Material materials with Shear modulus of 24.0 - 26.1 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

26.1 - 26.5 GPa

Show Material materials with Shear modulus of 26.1 - 26.5 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

Tensile strength

-196.0 °C

232.0 MPa

Show Material materials with Tensile strength of 232.0 MPa

O

EN 573-3

-80.0 °C

137.0 MPa

Show Material materials with Tensile strength of 137.0 MPa

O

EN 573-3

-20.0 °C

119.0 MPa

Show Material materials with Tensile strength of 119.0 MPa

O

EN 573-3

90.0 MPa

Show Material materials with Tensile strength of 90.0 MPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

95.0 MPa

Show Material materials with Tensile strength of 95.0 MPa

O

EN 573-3

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

130.0 MPa

Show Material materials with Tensile strength of 130.0 MPa

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

80.0 - 130.0 MPa

Show Material materials with Tensile strength of 80.0 - 130.0 MPa

O

EN 573-3, EN 546, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

90.0 - 130.0 MPa

Show Material materials with Tensile strength of 90.0 - 130.0 MPa

O

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Coil, Sheet

20.0 °C

90.0 MPa

Show Material materials with Tensile strength of 90.0 MPa

O

EN 573-3

Sheet

20.0 °C

90.0 - 130.0 MPa

Show Material materials with Tensile strength of 90.0 - 130.0 MPa

O

EN 573-3

Flat

Transverse

20.0 °C

95.0 - 130.0 MPa

Show Material materials with Tensile strength of 95.0 - 130.0 MPa

O

EN 573-3, EN 754

Rod, Tube, Strip, Sheet, Plate, Foil, Bar

20.0 °C

95.0 - 135.0 MPa

Show Material materials with Tensile strength of 95.0 - 135.0 MPa

O

EN 573-3, EN 755

Rod, Tube, Strip, Sheet, Plate, Foil, Bar

20.0 °C

95.0 MPa

Show Material materials with Tensile strength of 95.0 MPa

O

EN 573-3

Tube

20.0 °C

112.0 MPa

Show Material materials with Tensile strength of 112.0 MPa

O

EN 573-3

20.0 °C

130.0 MPa

Show Material materials with Tensile strength of 130.0 MPa

O

EN 573-3

Wire

100.0 °C

91.0 MPa

Show Material materials with Tensile strength of 91.0 MPa

O

EN 573-3

150.0 °C

77.0 MPa

Show Material materials with Tensile strength of 77.0 MPa

O

EN 573-3

200.0 °C

57.0 MPa

Show Material materials with Tensile strength of 57.0 MPa

O

EN 573-3

260.0 °C

47.0 MPa

Show Material materials with Tensile strength of 47.0 MPa

O

EN 573-3

320.0 °C

28.0 MPa

Show Material materials with Tensile strength of 28.0 MPa

O

EN 573-3

370.0 °C

19.0 MPa

Show Material materials with Tensile strength of 19.0 MPa

O

EN 573-3

Yield strength

-270 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat

RP02

-270.0 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat

RP02

-196.0 °C

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3

Wire

RP02

-80.0 °C

49.0 MPa

Show Material materials with Yield strength of 49.0 MPa

O

EN 573-3

RP02

-20.0 °C

46.0 MPa

Show Material materials with Yield strength of 46.0 MPa

O

EN 573-3

RP02

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3, EN 485, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

35 MPa

Show Material materials with Yield strength of 35 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3, EN 1301

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

O

EN 573-3, EN 683

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

RP02

20.0 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat

RP02

20 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat

RP02

20.0 °C

35.0 - 42.0 MPa

Show Material materials with Yield strength of 35.0 - 42.0 MPa

O

EN 573-3

RP02

20.0 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Flat

RP02 Transverse

20.0 °C

42.0 MPa

Show Material materials with Yield strength of 42.0 MPa

O

EN 573-3

RP02

20.0 °C

60.0 MPa

Show Material materials with Yield strength of 60.0 MPa

O

EN 573-3

Wire

RP02

20.0 °C

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

O

EN 573-3

Foil

RP02

50 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat

RP02

50.0 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat

RP02

100.0 °C

37.0 MPa

Show Material materials with Yield strength of 37.0 MPa

O

EN 573-3

RP02

150.0 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Rod, Tube, Sheet, Strip, Plate, Foil, Bar, Flat

RP02

200.0 °C

30.0 MPa

Show Material materials with Yield strength of 30.0 MPa

O

EN 573-3

RP02

260.0 °C

24.0 MPa

Show Material materials with Yield strength of 24.0 MPa

O

EN 573-3

RP02

320.0 °C

17.0 MPa

Show Material materials with Yield strength of 17.0 MPa

O

EN 573-3

RP02

370.0 °C

12.0 MPa

Show Material materials with Yield strength of 12.0 MPa

O

EN 573-3

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

100 °C

0.000025 1/K

Show Material materials with Coefficient of thermal expansion of 0.000025 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20-100°C

Melting point

645.0 - 655.0 °C

Show Material materials with Melting point of 645.0 - 655.0 °C

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

Specific heat capacity

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

20.0 °C

892.0 - 893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 892.0 - 893.0 J/(kg·K)

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

892.0 J/(kg·K)

Show Material materials with Specific heat capacity of 892.0 J/(kg·K)

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

893.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 J/(kg·K)

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

Thermal conductivity

176 W/(m·K)

Show Material materials with Thermal conductivity of 176 W/(m·K)

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

160.0 - 200.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 200.0 W/(m·K)

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

20.0 °C

160.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 W/(m·K)

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

22000000.0 - 28000000.0 S/m

Show Material materials with Electrical conductivity of 22000000.0 - 28000000.0 S/m

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire

20.0 °C

22000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 22000000.0 - 29000000.0 S/m

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

Electrical resistivity

3.57e-08 - 4.55e-08 Ω·m

Show Material materials with Electrical resistivity of 3.57e-08 - 4.55e-08 Ω·m

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

4.3e-08 Ω·m

Show Material materials with Electrical resistivity of 4.3e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

3.4e-08 - 4.1e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 4.1e-08 Ω·m

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

3.4e-08 - 4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.4e-08 - 4.5e-08 Ω·m

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

4.1e-08 Ω·m

Show Material materials with Electrical resistivity of 4.1e-08 Ω·m

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

20.0 °C

4.1e-08 - 4.5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.1e-08 - 4.5e-08 Ω·m

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar

0.1 %

Show Material materials with Chromium of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Copper

0.1 %

Show Material materials with Copper of 0.1 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar

0.1 %

Show Material materials with Copper of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Iron

0.7 %

Show Material materials with Iron of 0.7 %

O

EN 573-3

Foil, Rod, Sheet, Flat, Tube, Wire

0.70 %

Show Material materials with Iron of 0.70 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Foil, Bar, Rod, Tube

0.7 %

Show Material materials with Iron of 0.7 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Magnesium

0.3 %

Show Material materials with Magnesium of 0.3 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar

0.3 %

Show Material materials with Magnesium of 0.3 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Manganese

0.9 - 1.5 %

Show Material materials with Manganese of 0.9 - 1.5 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar, Coil, Sheet

Silicon

0.5 %

Show Material materials with Silicon of 0.5 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar

0.5 %

Show Material materials with Silicon of 0.5 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

O

EN 573-3, EN 1301, EN 485, EN 546, EN 683, EN 754, EN 755

Foil, Rod, Sheet, Flat, Tube, Wire, Strip, Plate, Bar

0.2 %

Show Material materials with Zinc of 0.2 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Technological properties

Property
Anodizing

decorative: sufficient, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Lithography; Heat exchangers: Fins, Heat exchangers; Tubes: Flexible tube, Pipes; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Components: Automotive fins, Heat exchangers

Brazing

hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good

Corrosion properties

Seawater: good, weathering: very good

Welding

Very Good

Workability