EN 573-3 Grade AW-3105 O

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMn alloy. The alloy is not food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

2.72 g/cm³

Show Material materials with Density of 2.72 g/cm³

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Flat, Coil, Sheet

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Coil, Sheet

2.0 mm

Show Material materials with Thickness of 2.0 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

2.0 mm

Coil, Sheet

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending angle 180°

0 °/t

Show Material materials with Bending angle 180° of 0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

Hardness, Brinell

29.0 [-]

Show Material materials with Hardness, Brinell of 29.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate

20.0 °C

29.0 [-]

Show Material materials with Hardness, Brinell of 29.0 [-]

O

EN 573-3

Flat

Hardness, HBW

29 [-]

Show Material materials with Hardness, HBW of 29 [-]

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Shear modulus

26.0 GPa

Show Material materials with Shear modulus of 26.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Tensile strength

20.0 °C

100.0 - 155.0 MPa

Show Material materials with Tensile strength of 100.0 - 155.0 MPa

O

EN 573-3

Sheet, Strip, Flat

Transverse

20.0 °C

100.0 - 155.0 MPa

Show Material materials with Tensile strength of 100.0 - 155.0 MPa

O

EN 573-3, EN 1396, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Coil, Sheet, Flat

Yield strength

40.0 MPa

Show Material materials with Yield strength of 40.0 MPa

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

RP02

40 MPa

Show Material materials with Yield strength of 40 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20.0 °C

40.0 MPa

Show Material materials with Yield strength of 40.0 MPa

O

EN 573-3

Sheet, Strip, Flat

RP02 Transverse

20.0 °C

40.0 MPa

Show Material materials with Yield strength of 40.0 MPa

O

EN 573-3

Sheet, Strip, Flat

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

20-100°C

Melting point

635.0 - 655.0 °C

Show Material materials with Melting point of 635.0 - 655.0 °C

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

640.0 - 655.0 °C

Show Material materials with Melting point of 640.0 - 655.0 °C

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

Specific heat capacity

893.0 - 920.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 - 920.0 J/(kg·K)

Typical for Wrought 3000 Series Aluminium

Thermal conductivity

160.0 - 190.0 W/(m·K)

Show Material materials with Thermal conductivity of 160.0 - 190.0 W/(m·K)

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

172 W/(m·K)

Show Material materials with Thermal conductivity of 172 W/(m·K)

O

EN 573-3, EN 1396, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Strip, Sheet, Plate, Coil, Sheet

20.0 °C

180.0 - 190.0 W/(m·K)

Show Material materials with Thermal conductivity of 180.0 - 190.0 W/(m·K)

O

EN 573-3

Sheet, Strip, Flat

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

23000000.0 - 26000000.0 S/m

Show Material materials with Electrical conductivity of 23000000.0 - 26000000.0 S/m

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

26000000.0 S/m

Show Material materials with Electrical conductivity of 26000000.0 S/m

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

20.0 °C

25000000.0 - 27000000.0 S/m

Show Material materials with Electrical conductivity of 25000000.0 - 27000000.0 S/m

O

EN 573-3

Sheet, Strip, Flat

Electrical resistivity

3.7999999999999996e-08 Ω·m

Show Material materials with Electrical resistivity of 3.7999999999999996e-08 Ω·m

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

3.85e-08 Ω·m

Show Material materials with Electrical resistivity of 3.85e-08 Ω·m

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

3.85e-08 - 4.35e-08 Ω·m

Show Material materials with Electrical resistivity of 3.85e-08 - 4.35e-08 Ω·m

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.2 %

Show Material materials with Chromium of 0.2 %

O

EN 573-3, EN 1396, EN 485

Sheet, Strip, Flat, Plate

0.2 %

Show Material materials with Chromium of 0.2 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Copper

0.3 %

Show Material materials with Copper of 0.3 %

O

EN 573-3, EN 1396, EN 485

Sheet, Strip, Flat, Plate

0.3 %

Show Material materials with Copper of 0.3 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Iron

0.7 %

Show Material materials with Iron of 0.7 %

O

EN 573-3

Sheet, Strip, Flat

0.70 %

Show Material materials with Iron of 0.70 %

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate

0.7 %

Show Material materials with Iron of 0.7 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Magnesium

0.2 - 0.8 %

Show Material materials with Magnesium of 0.2 - 0.8 %

O

EN 573-3, EN 1396, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Flat, Plate, Coil, Sheet

Manganese

0.3 - 0.8 %

Show Material materials with Manganese of 0.3 - 0.8 %

O

EN 573-3, EN 1396, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Sheet, Strip, Flat, Plate, Coil, Sheet

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

O

EN 573-3, EN 1396, EN 485

Sheet, Strip, Flat, Plate

0.6 %

Show Material materials with Silicon of 0.6 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

O

EN 573-3, EN 1396, EN 485

Sheet, Strip, Flat, Plate

Zinc

0.4 %

Show Material materials with Zinc of 0.4 %

O

EN 573-3, EN 1396, EN 485

Sheet, Strip, Flat, Plate

0.4 %

Show Material materials with Zinc of 0.4 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Coil, Sheet

Technological properties

Property
Anodizing

Good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Heat exchangers: Fins; Closures: Short cups; Semi-rigid and corrugated: Pet food

Brazing

hard brazing (with flux/ without flux): very good - acceptable / very good

Corrosion properties

Seawater: very good, weathering: very good

Surface Finish

Mill finish

Welding

Very Good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12)