EN 573-3 Grade AW-5005 O

Want to keep this datasheet? Save it now in your required format

Description

Aluminum EN AW-5005 is a lean aluminum magnesium alloy with low density and excellent thermal conductivity. This medium strength non-heat-treatable alloy is known for its corrosion resistance in alkaline marine situations. Aluminum EN AW-5005 is readily machinable, and can be welded using TIG and MIG methods. It is important to note that anodizing is a critical part to how Aluminum EN AW-5005 is used.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Coil, Sheet, Strip

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.1 mm

Show Material materials with Thickness of 0.1 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

0.1 mm

Coil, Sheet, Strip

4.0 mm

Show Material materials with Thickness of 4.0 mm

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

4.0 mm

Coil, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

70.0 MPa

Show Material materials with Bending Fatigue Strength of 70.0 MPa

O

EN 573-3, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Bending angle 180°

1.0 °/t

Show Material materials with Bending angle 180° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

0.5 °/t

Show Material materials with Bending angle 180° of 0.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

0 °/t

Show Material materials with Bending angle 180° of 0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Bending angle 90°

1.0 °/t

Show Material materials with Bending angle 90° of 1.0 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

0 °/t

Show Material materials with Bending angle 90° of 0 °/t

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Elastic modulus

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

O

EN 573-3

Sheet, Strip, Profile, Rod, Flat, Foil, Tube

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Elongation

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Sheet, Strip, Flat

A50 Transverse

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3

Sheet, Strip, Flat

A50 Transverse

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Sheet, Strip, Flat

A50 Transverse

20.0 °C

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3

Flat

A50 Transverse

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3

Rod, Tube

A50

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

O

EN 573-3

Foil

A50

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

O

EN 573-3

Foil

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3

Foil

A50

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Sheet, Strip, Flat

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3

Sheet, Strip, Flat

A50

20.0 °C

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3

Sheet, Strip, Flat

A50

20.0 °C

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3

Flat

A50

20.0 °C

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3

Flat

A50

19.0 %

Show Material materials with Elongation of 19.0 %

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

15.0 %

Show Material materials with Elongation of 15.0 %

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

24.0 %

Show Material materials with Elongation of 24.0 %

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

10.0 %

Show Material materials with Elongation of 10.0 %

O

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

8.0 %

Show Material materials with Elongation of 8.0 %

O

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

16.0 %

Show Material materials with Elongation of 16.0 %

O

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

15.0 - 22.0 %

Show Material materials with Elongation of 15.0 - 22.0 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

A50

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Profile, Tube, Rod, Flat

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3

Rod, Tube

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3

Flat

Transverse

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A100

18.0 %

Show Material materials with Elongation of 18.0 %

O

EN 573-3, EN 754

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A100

20.0 °C

8.0 %

Show Material materials with Elongation of 8.0 %

O

EN 573-3

Foil

A100

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

O

EN 573-3

Foil

A100

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

O

EN 573-3

Foil

A100

Hardness, Brinell

20.0 °C

30.0 [-]

Show Material materials with Hardness, Brinell of 30.0 [-]

O

EN 573-3

Profile, Rod, Tube

20.0 °C

29.0 [-]

Show Material materials with Hardness, Brinell of 29.0 [-]

O

EN 573-3

Flat

29.0 [-]

Show Material materials with Hardness, Brinell of 29.0 [-]

O

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Unlock all property charts

Hardness, HBW

29 [-]

Show Material materials with Hardness, HBW of 29 [-]

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

O

EN 573-3

Sheet, Strip, Profile, Rod, Flat, Foil, Tube

Shear modulus

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

O

EN 573-3

Sheet, Strip, Profile, Rod, Flat, Foil, Tube

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Tensile strength

20.0 °C

100.0 - 145.0 MPa

Show Material materials with Tensile strength of 100.0 - 145.0 MPa

O

EN 573-3

Sheet, Strip, Flat

Transverse

20.0 °C

100.0 - 150.0 MPa

Show Material materials with Tensile strength of 100.0 - 150.0 MPa

O

EN 573-3, EN 755

Profile, Rod, Tube, Foil, Strip, Sheet, Plate, Welded Tube, Bar

20.0 °C

100.0 - 145.0 MPa

Show Material materials with Tensile strength of 100.0 - 145.0 MPa

O

EN 573-3, EN 1396, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Rod, Tube, Sheet, Strip, Flat, Plate, Welded Tube, Bar, Coil, Sheet, Strip

20.0 °C

90.0 - 145.0 MPa

Show Material materials with Tensile strength of 90.0 - 145.0 MPa

O

EN 573-3, EN 683

Foil, Strip, Sheet, Plate, Tube, Welded Tube, Bar

Unlock all property charts

Yield strength

20.0 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Sheet, Strip, Flat

RP02 Transverse

20.0 °C

40.0 MPa

Show Material materials with Yield strength of 40.0 MPa

O

EN 573-3

Profile, Rod, Tube

RP02

20.0 °C

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

O

EN 573-3

Foil

RP02

20.0 °C

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3

Sheet, Strip, Flat

RP02

35.0 MPa

Show Material materials with Yield strength of 35.0 MPa

O

EN 573-3, EN 1396, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

RP02

80.0 MPa

Show Material materials with Yield strength of 80.0 MPa

O

EN 573-3, EN 683

Strip, Sheet, Plate, Tube, Welded Tube, Bar

RP02

40.0 MPa

Show Material materials with Yield strength of 40.0 MPa

O

EN 573-3, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

RP02

35 MPa

Show Material materials with Yield strength of 35 MPa

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Unlock all property charts

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

20-100°C

100 °C, 20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Unlock all property charts

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

630.0 - 655.0 °C

Show Material materials with Melting point of 630.0 - 655.0 °C

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Specific heat capacity

20.0 °C

897.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 J/(kg·K)

O

EN 573-3

Sheet, Strip, Profile, Rod, Flat, Foil, Tube

Thermal conductivity

20.0 °C

201.0 W/(m·K)

Show Material materials with Thermal conductivity of 201.0 W/(m·K)

O

EN 573-3

Sheet, Strip, Profile, Rod, Flat, Foil, Tube

201 W/(m·K)

Show Material materials with Thermal conductivity of 201 W/(m·K)

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

200 W/(m·K)

Show Material materials with Thermal conductivity of 200 W/(m·K)

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

30000000.0 S/m

Show Material materials with Electrical conductivity of 30000000.0 S/m

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Electrical resistivity

20.0 °C

3.3e-08 Ω·m

Show Material materials with Electrical resistivity of 3.3e-08 Ω·m

O

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Coil, Sheet, Strip

3.33e-08 Ω·m

Show Material materials with Electrical resistivity of 3.33e-08 Ω·m

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar

0.1 %

Show Material materials with Chromium of 0.1 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Copper

0.2 %

Show Material materials with Copper of 0.2 %

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar

0.05 %

Show Material materials with Copper of 0.05 %

O

EN 573-3

Rod, Tube

0.2 %

Show Material materials with Copper of 0.2 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Iron

0.7 %

Show Material materials with Iron of 0.7 %

O

EN 573-3

Sheet, Strip, Profile, Rod, Flat, Foil, Tube

0.45 %

Show Material materials with Iron of 0.45 %

O

EN 573-3

Rod, Tube

0.70 %

Show Material materials with Iron of 0.70 %

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Strip, Sheet, Plate, Tube, Welded Tube, Bar

0.7 %

Show Material materials with Iron of 0.7 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Magnesium

0.5 - 1.1 %

Show Material materials with Magnesium of 0.5 - 1.1 %

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar, Coil, Sheet, Strip

0.7 - 1.1 %

Show Material materials with Magnesium of 0.7 - 1.1 %

O

EN 573-3

Rod, Tube

Manganese

0.2 %

Show Material materials with Manganese of 0.2 %

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar

0.15 %

Show Material materials with Manganese of 0.15 %

O

EN 573-3

Rod, Tube

0.2 %

Show Material materials with Manganese of 0.2 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Silicon

0.3 %

Show Material materials with Silicon of 0.3 %

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar

0.3 %

Show Material materials with Silicon of 0.3 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

O

EN 573-3, EN 1396, EN 485, EN 683, EN 754, EN 755

Sheet, Strip, Profile, Rod, Flat, Foil, Tube, Plate, Welded Tube, Bar

0.2 %

Show Material materials with Zinc of 0.2 %

O

EN 573-3

Rod, Tube

0.25 %

Show Material materials with Zinc of 0.25 %

O

EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2

Coil, Sheet, Strip

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Application areas

Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Heat exchangers: Fins, General applications; Cosmetics: Cosmetics pieces; Automotive trim: Interior trim; Components: Automotive fins, Heat exchangers

Brazing

hard brazing (with flux/ without flux): acceptable / sufficient, friction soldering: good, soft brazing with flux: sufficient

Corrosion properties

Seawater: good, weathering: very good

Welding

Very Good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (O)