Aluminum EN AW-5005 is a lean aluminum magnesium alloy with low density and excellent thermal conductivity. This medium strength non-heat-treatable alloy is known for its corrosion resistance in alkaline marine situations. Aluminum EN AW-5005 is readily machinable, and can be welded using TIG and MIG methods. It is important to note that anodizing is a critical part to how Aluminum EN AW-5005 is used.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H28

EN 573-3

Flat, Seamless Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Bending Fatigue Strength

80.0 MPa

Show Material materials with Bending Fatigue Strength of 80.0 MPa

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Bending angle 90°

1.5 °/t

Show Material materials with Bending angle 90° of 1.5 °/t

H28

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

2.5 °/t

Show Material materials with Bending angle 90° of 2.5 °/t

H28

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

3.0 °/t

Show Material materials with Bending angle 90° of 3.0 °/t

H28

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

69.5 GPa

Show Material materials with Elastic modulus of 69.5 GPa

H28

EN 573-3

Flat, Seamless Tube

Elongation

1.0 %

Show Material materials with Elongation of 1.0 %

H28

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

2.0 %

Show Material materials with Elongation of 2.0 %

H28

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

3.0 %

Show Material materials with Elongation of 3.0 %

H28

EN 573-3, EN 1592

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A100

3.0 %

Show Material materials with Elongation of 3.0 %

H28

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

A50

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H28

EN 573-3

Flat

A50 Transverse

20.0 °C

1.0 %

Show Material materials with Elongation of 1.0 %

H28

EN 573-3

Flat

A50

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H28

EN 573-3

Flat

A50 Transverse

20.0 °C

2.0 %

Show Material materials with Elongation of 2.0 %

H28

EN 573-3

Flat

A50

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H28

EN 573-3

Flat

A50 Transverse

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H28

EN 573-3

Seamless Tube

20.0 °C

3.0 %

Show Material materials with Elongation of 3.0 %

H28

EN 573-3

Flat

A50

Hardness, Brinell

58.0 [-]

Show Material materials with Hardness, Brinell of 58.0 [-]

H28

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

58.0 [-]

Show Material materials with Hardness, Brinell of 58.0 [-]

H28

EN 573-3

Flat

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

20.0 °C

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

H28

EN 573-3

Flat, Seamless Tube

Shear modulus

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

26.1 GPa

Show Material materials with Shear modulus of 26.1 GPa

H28

EN 573-3

Flat, Seamless Tube

Tensile strength

185.0 MPa

Show Material materials with Tensile strength of 185.0 MPa

H28

EN 573-3, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H28

EN 573-3, EN 1592

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

185.0 MPa

Show Material materials with Tensile strength of 185.0 MPa

H28

EN 573-3

Flat

Transverse

20.0 °C

185.0 MPa

Show Material materials with Tensile strength of 185.0 MPa

H28

EN 573-3

Flat

20.0 °C

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H28

EN 573-3

Seamless Tube

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

630.0 - 655.0 °C

Show Material materials with Melting point of 630.0 - 655.0 °C

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Specific heat capacity

20.0 °C

897.0 J/(kg·K)

Show Material materials with Specific heat capacity of 897.0 J/(kg·K)

H28

EN 573-3

Flat, Seamless Tube

Thermal conductivity

201 W/(m·K)

Show Material materials with Thermal conductivity of 201 W/(m·K)

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

201.0 W/(m·K)

Show Material materials with Thermal conductivity of 201.0 W/(m·K)

H28

EN 573-3

Flat, Seamless Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

30000000.0 S/m

Show Material materials with Electrical conductivity of 30000000.0 S/m

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Electrical resistivity

3.33e-08 Ω·m

Show Material materials with Electrical resistivity of 3.33e-08 Ω·m

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

20.0 °C

3.3e-08 Ω·m

Show Material materials with Electrical resistivity of 3.3e-08 Ω·m

H28

EN 573-3

Flat, Seamless Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H28

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Tube, Welded Tube, Bar

Copper

0.2 %

Show Material materials with Copper of 0.2 %

H28

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Tube, Welded Tube, Bar

Iron

0.7 %

Show Material materials with Iron of 0.7 %

H28

EN 573-3

Flat, Seamless Tube

0.70 %

Show Material materials with Iron of 0.70 %

H28

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Tube, Welded Tube, Bar

Magnesium

0.5 - 1.1 %

Show Material materials with Magnesium of 0.5 - 1.1 %

H28

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Tube, Welded Tube, Bar

Manganese

0.2 %

Show Material materials with Manganese of 0.2 %

H28

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Tube, Welded Tube, Bar

Silicon

0.3 %

Show Material materials with Silicon of 0.3 %

H28

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Tube, Welded Tube, Bar

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H28

EN 573-3, EN 1592, EN 485

Flat, Seamless Tube, Strip, Sheet, Plate, Tube, Welded Tube, Bar

Technological properties

Property
Anodizing

decorative: acceptable, Protective: very good

Brazing

hard brazing (with flux/ without flux): acceptable / sufficient, friction soldering: good, soft brazing with flux: sufficient

Corrosion properties

Seawater: good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (O)