General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
20.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | H111 | EN 573-3 | Profile, Rod, Flat, Tube |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending angle 180° | 0.5 °/t Show Material materials with Bending angle 180° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
1.0 °/t Show Material materials with Bending angle 180° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
Bending angle 90° | 1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
69.5 GPa Show Material materials with Elastic modulus of 69.5 GPa | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
20.0 °C | 69.5 GPa Show Material materials with Elastic modulus of 69.5 GPa | H111 | EN 573-3 | Profile, Rod, Flat, Tube | ||
Elongation | 15.0 % Show Material materials with Elongation of 15.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | |
16.0 % Show Material materials with Elongation of 16.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
18.0 % Show Material materials with Elongation of 18.0 % | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
18.0 % Show Material materials with Elongation of 18.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A100 | ||
19.0 % Show Material materials with Elongation of 19.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
20.0 % Show Material materials with Elongation of 20.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
20.0 % Show Material materials with Elongation of 20.0 % | H111 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A100 | ||
22.0 % Show Material materials with Elongation of 22.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
24.0 % Show Material materials with Elongation of 24.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
20.0 °C | 15.0 % Show Material materials with Elongation of 15.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 15.0 % Show Material materials with Elongation of 15.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | H111 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | H111 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 19.0 % Show Material materials with Elongation of 19.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 19.0 % Show Material materials with Elongation of 19.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Elongation of 20.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 20.0 % Show Material materials with Elongation of 20.0 % | H111 | EN 573-3 | Profile, Tube, Rod, Flat | ||
20.0 °C | 20.0 % Show Material materials with Elongation of 20.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Elongation of 20.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 22.0 % Show Material materials with Elongation of 22.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 22.0 % Show Material materials with Elongation of 22.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 24.0 % Show Material materials with Elongation of 24.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 24.0 % Show Material materials with Elongation of 24.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
Hardness, Brinell | 29.0 [-] Show Material materials with Hardness, Brinell of 29.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 29.0 [-] Show Material materials with Hardness, Brinell of 29.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 30.0 [-] Show Material materials with Hardness, Brinell of 30.0 [-] | H111 | EN 573-3 | Profile, Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poisson's ratio | 20.0 °C | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | H111 | EN 573-3 | Profile, Rod, Flat, Tube | |
Shear modulus | 26.1 GPa Show Material materials with Shear modulus of 26.1 GPa | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 26.1 GPa Show Material materials with Shear modulus of 26.1 GPa | H111 | EN 573-3 | Profile, Rod, Flat, Tube | ||
Tensile strength | 20.0 °C | 100.0 - 150.0 MPa Show Material materials with Tensile strength of 100.0 - 150.0 MPa | H111 | EN 573-3, EN 755 | Profile, Rod, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
20.0 °C | 100.0 - 145.0 MPa Show Material materials with Tensile strength of 100.0 - 145.0 MPa | H111 | EN 573-3, EN 485, EN 754 | Rod, Tube, Flat, Strip, Sheet, Plate, Welded Tube, Bar | ||
20.0 °C | 100.0 - 145.0 MPa Show Material materials with Tensile strength of 100.0 - 145.0 MPa | H111 | EN 573-3 | Flat | Transverse |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
100 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Melting point | 630.0 - 655.0 °C Show Material materials with Melting point of 630.0 - 655.0 °C | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Specific heat capacity | 20.0 °C | 897.0 J/(kg·K) Show Material materials with Specific heat capacity of 897.0 J/(kg·K) | H111 | EN 573-3 | Profile, Rod, Flat, Tube | |
Thermal conductivity | 201 W/(m·K) Show Material materials with Thermal conductivity of 201 W/(m·K) | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 201.0 W/(m·K) Show Material materials with Thermal conductivity of 201.0 W/(m·K) | H111 | EN 573-3 | Profile, Rod, Flat, Tube |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 30000000.0 S/m Show Material materials with Electrical conductivity of 30000000.0 S/m | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
Electrical resistivity | 3.33e-08 Ω·m Show Material materials with Electrical resistivity of 3.33e-08 Ω·m | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
20.0 °C | 3.3e-08 Ω·m Show Material materials with Electrical resistivity of 3.3e-08 Ω·m | H111 | EN 573-3 | Profile, Rod, Flat, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
Copper | 0.05 % Show Material materials with Copper of 0.05 % | H111 | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Copper of 0.2 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
Iron | 0.45 % Show Material materials with Iron of 0.45 % | H111 | EN 573-3 | Rod, Tube |
0.7 % Show Material materials with Iron of 0.7 % | H111 | EN 573-3 | Profile, Rod, Flat, Tube | |
0.70 % Show Material materials with Iron of 0.70 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
Magnesium | 0.5 - 1.1 % Show Material materials with Magnesium of 0.5 - 1.1 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
0.7 - 1.1 % Show Material materials with Magnesium of 0.7 - 1.1 % | H111 | EN 573-3 | Rod, Tube | |
Manganese | 0.15 % Show Material materials with Manganese of 0.15 % | H111 | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Manganese of 0.2 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
Silicon | 0.3 % Show Material materials with Silicon of 0.3 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H111 | EN 573-3 | Rod, Tube |
0.25 % Show Material materials with Zinc of 0.25 % | H111 | EN 573-3, EN 485, EN 754, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): acceptable / sufficient, friction soldering: good, soft brazing with flux: sufficient | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (O) |