EN 573-3 Grade AW-5049 H112

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H112

EN 573-3

Profile, Rod, Sheet, Flat, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-270 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H112

EN 573-3

Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H112

EN 573-3

Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

20 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H112

EN 573-3

Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H112

EN 573-3

Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H112

EN 573-3

Profile, Rod, Sheet, Flat, Tube

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H112

EN 573-3

Profile, Rod, Sheet, Flat, Tube

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H112

EN 573-3

Profile, Rod, Sheet, Flat, Tube

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H112

EN 573-3

Profile, Rod, Sheet, Flat, Tube

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H112

EN 573-3

Profile, Rod, Sheet, Flat, Tube

300 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H112

EN 573-3

Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H112

EN 573-3

Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat

Elongation

10.0 %

Show Material materials with Elongation of 10.0 %

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A100

12.0 %

Show Material materials with Elongation of 12.0 %

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A50

12.0 %

Show Material materials with Elongation of 12.0 %

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A100

13.0 %

Show Material materials with Elongation of 13.0 %

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A50

14.0 %

Show Material materials with Elongation of 14.0 %

H112

EN 573-3

Strip, Sheet, Plate, Rod, Tube, Welded Tube

14.0 %

Show Material materials with Elongation of 14.0 %

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A100

15.0 %

Show Material materials with Elongation of 15.0 %

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A100

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H112

EN 573-3

Flat

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H112

EN 573-3

Flat

Transverse

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

H112

EN 573-3

Flat

A50 Transverse

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

H112

EN 573-3

Flat

A50

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

H112

EN 573-3

Sheet

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

H112

EN 573-3

Flat

Transverse

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

H112

EN 573-3

Profile, Rod, Tube

A50

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H112

EN 573-3

A50 Transverse

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H112

EN 573-3

Rod, Sheet, Tube, Profile

20.0 °C

14.0 %

Show Material materials with Elongation of 14.0 %

H112

EN 573-3

Flat

Transverse

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

H112

EN 573-3

Rod, Tube, Profile

Hardness, Brinell

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

52.0 [-]

Show Material materials with Hardness, Brinell of 52.0 [-]

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

58.0 [-]

Show Material materials with Hardness, Brinell of 58.0 [-]

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

62.0 [-]

Show Material materials with Hardness, Brinell of 62.0 [-]

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

20.0 °C

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

H112

EN 573-3

Profile, Rod, Tube

20.0 °C

52.0 [-]

Show Material materials with Hardness, Brinell of 52.0 [-]

H112

EN 573-3

Flat, Sheet

20.0 °C

52.0 - 62.0 [-]

Show Material materials with Hardness, Brinell of 52.0 - 62.0 [-]

H112

EN 573-3

Flat

20.0 °C

52.0 - 58.0 [-]

Show Material materials with Hardness, Brinell of 52.0 - 58.0 [-]

H112

EN 573-3

Flat, Sheet

20.0 °C

58.0 - 62.0 [-]

Show Material materials with Hardness, Brinell of 58.0 - 62.0 [-]

H112

EN 573-3

Flat

20.0 °C

58.0 [-]

Show Material materials with Hardness, Brinell of 58.0 [-]

H112

EN 573-3

Flat, Sheet

20.0 °C

62.0 [-]

Show Material materials with Hardness, Brinell of 62.0 [-]

H112

EN 573-3

Flat

Impact strength, Charpy notched

30.0 kJ/m²

Show Material materials with Impact strength, Charpy notched of 30.0 kJ/m²

H112

EN 573-3

Strip, Sheet, Plate, Rod, Tube, Welded Tube

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

20.0 °C

26.5

Show Material materials with Shear modulus of 26.5

H112

EN 573-3

Profile, Rod, Sheet, Flat, Tube

Tensile strength

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

H112

EN 573-3, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

210.0 MPa

Show Material materials with Tensile strength of 210.0 MPa

H112

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

20.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

H112

EN 573-3

Rod, Tube, Profile

20.0 °C

190.0 - 240.0 MPa

Show Material materials with Tensile strength of 190.0 - 240.0 MPa

H112

EN 573-3

Transverse

20.0 °C

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H112

EN 573-3

Flat

Transverse

20.0 °C

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

H112

EN 573-3

Sheet

20.0 °C

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H112

EN 573-3

Flat

Transverse

20.0 °C

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H112

EN 573-3

Rod, Tube, Profile, Flat

20.0 °C

210.0 MPa

Show Material materials with Tensile strength of 210.0 MPa

H112

EN 573-3

Flat

Transverse

20.0 °C

210.0 MPa

Show Material materials with Tensile strength of 210.0 MPa

H112

EN 573-3

Flat

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

100 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

H112

EN 573-3

Profile, Rod, Sheet, Flat, Tube

Long

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

620.0 - 650.0 °C

Show Material materials with Melting point of 620.0 - 650.0 °C

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

Specific heat capacity

879.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K)

Typical for Wrought 5000 Series Aluminium

Thermal conductivity

20.0 °C

140.0 - 180.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 180.0 W/(m·K)

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

20000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 25000000.0 S/m

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube

Electrical resistivity

4e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4e-08 - 5e-08 Ω·m

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube

Iron

0.5 %

Show Material materials with Iron of 0.5 %

H112

EN 573-3

Profile, Rod, Sheet, Flat, Tube

0.50 %

Show Material materials with Iron of 0.50 %

H112

EN 573-3, EN 485, EN 755

Strip, Sheet, Plate, Rod, Tube, Welded Tube

Magnesium

1.6 - 2.5 %

Show Material materials with Magnesium of 1.6 - 2.5 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube

Manganese

0.5 - 1.1 %

Show Material materials with Manganese of 0.5 - 1.1 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H112

EN 573-3, EN 485, EN 755

Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12)