EN 573-3 Grade AW-5049 H12

Want to keep this datasheet? Save it now in your required format

Description

Naturally hard AlMg alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey,Aludium.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H12

EN 573-3, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

H12

EN 573-3

Flat, Seamless Tube, Tube

Dimension

PropertyValueConditionRelated StandardsThicknessShape

Thickness

0.2 mm

Show Material materials with Thickness of 0.2 mm

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

0.2 mm

Plate, Sheet, Strip

6.0 mm

Show Material materials with Thickness of 6.0 mm

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

6.0 mm

Plate, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

-270.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Seamless Tube, Tube, Plate, Sheet, Strip

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

H12

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Seamless Tube, Tube, Plate, Sheet, Strip

50.0 °C

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H12

EN 573-3

Flat, Seamless Tube, Tube

100.0 °C

68.0 GPa

Show Material materials with Elastic modulus of 68.0 GPa

H12

EN 573-3

Flat, Seamless Tube, Tube

150.0 °C

66.0 GPa

Show Material materials with Elastic modulus of 66.0 GPa

H12

EN 573-3

Flat, Seamless Tube, Tube

200.0 °C

63.0 GPa

Show Material materials with Elastic modulus of 63.0 GPa

H12

EN 573-3

Flat, Seamless Tube, Tube

250.0 °C

57.0 GPa

Show Material materials with Elastic modulus of 57.0 GPa

H12

EN 573-3

Flat, Seamless Tube, Tube

300.0 °C

50.0 GPa

Show Material materials with Elastic modulus of 50.0 GPa

H12

EN 573-3

Flat, Seamless Tube, Tube

Elongation

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A50

4.0 - 7.0 %

Show Material materials with Elongation of 4.0 - 7.0 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

A50

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A50

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A50

7.0 %

Show Material materials with Elongation of 7.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A50

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A50

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A100

10.0 %

Show Material materials with Elongation of 10.0 %

H12

EN 573-3, EN 1592, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

A100

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

4.0 %

Show Material materials with Elongation of 4.0 %

H12

EN 573-3

Flat

A50

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

5.0 %

Show Material materials with Elongation of 5.0 %

H12

EN 573-3

Flat

A50

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

6.0 %

Show Material materials with Elongation of 6.0 %

H12

EN 573-3

Flat

A50

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

7.0 %

Show Material materials with Elongation of 7.0 %

H12

EN 573-3

Flat

A50

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Flat

A50 Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Flat

Transverse

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Flat

20.0 °C

9.0 %

Show Material materials with Elongation of 9.0 %

H12

EN 573-3

Tube, Flat

A50

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

H12

EN 573-3

Seamless Tube, Tube

Hardness, Brinell

65.0 [-]

Show Material materials with Hardness, Brinell of 65.0 [-]

H12

EN 573-3, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

66.0 [-]

Show Material materials with Hardness, Brinell of 66.0 [-]

H12

EN 573-3, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

20.0 °C

52.0 [-]

Show Material materials with Hardness, Brinell of 52.0 [-]

H12

EN 573-3

Flat

20.0 °C

52.0 - 66.0 [-]

Show Material materials with Hardness, Brinell of 52.0 - 66.0 [-]

H12

EN 573-3

Flat

20.0 °C

65.0 [-]

Show Material materials with Hardness, Brinell of 65.0 [-]

H12

EN 573-3

Tube

20.0 °C

66.0 [-]

Show Material materials with Hardness, Brinell of 66.0 [-]

H12

EN 573-3

Flat

Hardness, HBW

66 [-]

Show Material materials with Hardness, HBW of 66 [-]

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

20.0 °C

26.5 GPa

Show Material materials with Shear modulus of 26.5 GPa

H12

EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Seamless Tube, Tube, Plate, Sheet, Strip

Tensile strength

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

H12

EN 573-3, EN 1592

Strip, Sheet, Plate, Rod, Tube, Welded Tube

20.0 °C

210.0 - 270.0 MPa

Show Material materials with Tensile strength of 210.0 - 270.0 MPa

H12

EN 573-3, EN 754

Tube, Strip, Sheet, Plate, Rod, Welded Tube

20.0 °C

220.0 - 270.0 MPa

Show Material materials with Tensile strength of 220.0 - 270.0 MPa

H12

EN 573-3

Flat

Transverse

20.0 °C

220.0 MPa

Show Material materials with Tensile strength of 220.0 MPa

H12

EN 573-3

Seamless Tube

20.0 °C

220.0 - 270.0 MPa

Show Material materials with Tensile strength of 220.0 - 270.0 MPa

H12

EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Strip, Sheet, Plate, Rod, Tube, Welded Tube, Sheet, Strip

Yield strength

120.0 MPa

Show Material materials with Yield strength of 120.0 MPa

H12

EN 573-3, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

RP02

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H12

EN 573-3, EN 1592, EN 485

Strip, Sheet, Plate, Rod, Tube, Welded Tube

RP02

170 MPa

Show Material materials with Yield strength of 170 MPa

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

20.0 °C

120.0 MPa

Show Material materials with Yield strength of 120.0 MPa

H12

EN 573-3

Tube

RP02

20.0 °C

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H12

EN 573-3

Flat

RP02 Transverse

20.0 °C

170.0 MPa

Show Material materials with Yield strength of 170.0 MPa

H12

EN 573-3

Seamless Tube, Flat

RP02

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H12

EN 573-3, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

100 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

H12

EN 573-3, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

100 °C

0.000024 1/K

Show Material materials with Coefficient of thermal expansion of 0.000024 1/K

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

20-100°C

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

H12

EN 573-3

Flat, Seamless Tube, Tube

Long

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

620.0 - 650.0 °C

Show Material materials with Melting point of 620.0 - 650.0 °C

H12

EN 573-3, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

Specific heat capacity

879.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K)

Typical for Wrought 5000 Series Aluminium

Thermal conductivity

147 W/(m·K)

Show Material materials with Thermal conductivity of 147 W/(m·K)

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

20.0 °C

140.0 - 180.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 180.0 W/(m·K)

H12

EN 573-3, EN 1592, EN 485, EN 754

Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Rod, Welded Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

20000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 25000000.0 S/m

H12

EN 573-3, EN 1592, EN 485, EN 754

Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Rod, Welded Tube

Electrical resistivity

4e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4e-08 - 5e-08 Ω·m

H12

EN 573-3, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

4.4e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4.4e-08 - 5e-08 Ω·m

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

H12

EN 573-3, EN 1592, EN 485, EN 754

Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Rod, Welded Tube

0.3 %

Show Material materials with Chromium of 0.3 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

Copper

0.1 %

Show Material materials with Copper of 0.1 %

H12

EN 573-3, EN 1592, EN 485, EN 754

Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Rod, Welded Tube

0.1 %

Show Material materials with Copper of 0.1 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

Iron

0.5 %

Show Material materials with Iron of 0.5 %

H12

EN 573-3

Flat, Seamless Tube, Tube

0.50 %

Show Material materials with Iron of 0.50 %

H12

EN 573-3, EN 1592, EN 485, EN 754

Strip, Sheet, Plate, Rod, Tube, Welded Tube

0.5 %

Show Material materials with Iron of 0.5 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

Magnesium

1.6 - 2.5 %

Show Material materials with Magnesium of 1.6 - 2.5 %

H12

EN 573-3, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Rod, Welded Tube, Sheet, Strip

Manganese

0.5 - 1.1 %

Show Material materials with Manganese of 0.5 - 1.1 %

H12

EN 573-3, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2

Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Rod, Welded Tube, Sheet, Strip

Other

0.05 - 0.15 %

Show Material materials with Other of 0.05 - 0.15 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

H12

EN 573-3, EN 1592, EN 485, EN 754

Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Rod, Welded Tube

0.4 %

Show Material materials with Silicon of 0.4 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

H12

EN 573-3, EN 1592, EN 485, EN 754

Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Rod, Welded Tube

0.1 %

Show Material materials with Titanium of 0.1 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

H12

EN 573-3, EN 1592, EN 485, EN 754

Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Rod, Welded Tube

0.2 %

Show Material materials with Zinc of 0.2 %

H12

EN 573-1, EN 573-2, EN 573-3, EN 485-2

Plate, Sheet, Strip

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Application areas

Components: General trasportation

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Welding

Very Good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12)