General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.72 g/cm³ Show Material materials with Density of 2.72 g/cm³ | H14 | EN 573-3, EN 1592, EN 485 | ||
20.0 °C | 2.72 g/cm³ Show Material materials with Density of 2.72 g/cm³ | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending angle 180° | 2.5 °/t Show Material materials with Bending angle 180° of 2.5 °/t | H14 | EN 573-3, EN 485 | |||
Bending angle 90° | 0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | ||||
1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | H14 | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | H14 | EN 573-3, EN 485 | ||||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H14 | EN 573-3, EN 1592, EN 485 | |||
70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H14 | EN 573-3, EN 1592, EN 485 | ||||
20.0 °C | 65.0 - 71.0 GPa Show Material materials with Elastic modulus of 65.0 - 71.0 GPa | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Elongation | 1.0 % Show Material materials with Elongation of 1.0 % | H14 | EN 573-3, EN 485 | A50 | ||
2.0 % Show Material materials with Elongation of 2.0 % | H14 | EN 573-3, EN 485 | A50 | |||
3.0 % Show Material materials with Elongation of 3.0 % | H14 | EN 573-3, EN 485 | A50 | |||
6.0 % Show Material materials with Elongation of 6.0 % | H14 | EN 573-3, EN 1592 | A100 | |||
20.0 °C | 3.0 % Show Material materials with Elongation of 3.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Hardness, Brinell | 67.0 [-] Show Material materials with Hardness, Brinell of 67.0 [-] | H14 | EN 573-3, EN 485 | |||
20.0 °C | 65.0 [-] Show Material materials with Hardness, Brinell of 65.0 [-] | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 25.0 - 27.0 GPa Show Material materials with Shear modulus of 25.0 - 27.0 GPa | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
Tensile strength | 220.0 MPa Show Material materials with Tensile strength of 220.0 MPa | H14 | EN 573-3, EN 1592 | |||
220.0 - 265.0 MPa Show Material materials with Tensile strength of 220.0 - 265.0 MPa | H14 | EN 573-3, EN 485 | ||||
20.0 °C | 220.0 - 260.0 MPa Show Material materials with Tensile strength of 220.0 - 260.0 MPa | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K | H14 | EN 573-3, EN 1592, EN 485 | |
-50.0 °C | 2.15e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.15e-05 1/K | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.1499999999999997e-05 1/K | H14 | EN 573-3, EN 1592, EN 485 | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H14 | EN 573-3, EN 1592, EN 485 | ||
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K | H14 | EN 573-3, EN 1592, EN 485 | ||
20 °C | 2.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K | H14 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
20 °C | 2.51e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K | H14 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K | H14 | EN 573-3, EN 1592, EN 485 | ||
100.0 °C | 2.32e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.32e-05 1/K | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K | H14 | EN 573-3, EN 1592, EN 485 | ||
200 °C | 2.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K | H14 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
200.0 °C | 2.41e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.41e-05 1/K | H14 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
300 °C | 2.51e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K | H14 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
300.0 °C | 2.51e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.51e-05 1/K | H14 | EN 573-3, EN 1592, EN 485, DIN 1725-1, EN 573-4 | Flat | |
Melting point | 629.0 - 654.0 °C Show Material materials with Melting point of 629.0 - 654.0 °C | H14 | EN 573-3, EN 1592, EN 485 | ||
630.0 - 655.0 °C Show Material materials with Melting point of 630.0 - 655.0 °C | H14 | EN 573-3, EN 1592, EN 485 | |||
Specific heat capacity | 893.0 J/(kg·K) Show Material materials with Specific heat capacity of 893.0 J/(kg·K) | H14 | EN 573-3, EN 1592, EN 485 | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Specific heat capacity of 893.0 J/(kg·K) | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
Thermal conductivity | 160.0 - 180.0 W/(m·K) Show Material materials with Thermal conductivity of 160.0 - 180.0 W/(m·K) | H14 | EN 573-3, EN 1592, EN 485 | ||
163 W/(m·K) Show Material materials with Thermal conductivity of 163 W/(m·K) | H14 | EN 573-3, EN 1592, EN 485 | |||
20.0 °C | 160.0 - 190.0 W/(m·K) Show Material materials with Thermal conductivity of 160.0 - 190.0 W/(m·K) | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 23000000.0 - 25000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 25000000.0 S/m | H14 | EN 573-3, EN 1592, EN 485 | ||
24000000.0 S/m Show Material materials with Electrical conductivity of 24000000.0 S/m | H14 | EN 573-3, EN 1592, EN 485 | |||
20.0 °C | 20000000.0 - 24000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 - 24000000.0 S/m | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat | |
Electrical resistivity | 4e-08 - 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 4e-08 - 4.35e-08 Ω·m | H14 | EN 573-3, EN 1592, EN 485 | ||
4.17e-08 Ω·m Show Material materials with Electrical resistivity of 4.17e-08 Ω·m | H14 | EN 573-3, EN 1592, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Copper | 0.25 % Show Material materials with Copper of 0.25 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | H14 | DIN 1725-1, EN 573-3, EN 573-4 | Flat |
0.70 % Show Material materials with Iron of 0.70 % | H14 | EN 573-3, EN 1592, EN 485 | ||
Magnesium | 0.8 - 1.3 % Show Material materials with Magnesium of 0.8 - 1.3 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Manganese | 1.0 - 1.5 % Show Material materials with Manganese of 1.0 - 1.5 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Silicon | 0.3 % Show Material materials with Silicon of 0.3 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H14 | DIN 1725-1, EN 573-3, EN 573-4, EN 1592, EN 485 | Flat |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12) |