General
Property | Value | Condition | Related Standards |
---|---|---|---|
Density | 2.68 g/cm³ Show Material materials with Density of 2.68 g/cm³ | H12 | EN 573-3, EN 485 |
2.69 g/cm³ Show Material materials with Density of 2.69 g/cm³ | H12 | EN 573-3, EN 485 |
Mechanical
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending angle 90° | 0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H12 | EN 573-3, EN 485 | |
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H12 | EN 573-3, EN 485 | ||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H12 | EN 573-3, EN 485 | |
70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H12 | EN 573-3, EN 485 | ||
Hardness, Brinell | 49.0 [-] Show Material materials with Hardness, Brinell of 49.0 [-] | H12 | EN 573-3, EN 485 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Shear modulus | 26.0 - 26.5 GPa Show Material materials with Shear modulus of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||
Tensile strength | 155.0 - 195.0 MPa Show Material materials with Tensile strength of 155.0 - 195.0 MPa | H12 | EN 573-3, EN 485 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H12 | EN 573-3, EN 485 | |
100 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H12 | EN 573-3, EN 485 | ||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Melting point | 620.0 - 650.0 °C Show Material materials with Melting point of 620.0 - 650.0 °C | H12 | EN 573-3, EN 485 | ||
625.0 - 650.0 °C Show Material materials with Melting point of 625.0 - 650.0 °C | H12 | EN 573-3, EN 485 | |||
Specific heat capacity | 879.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | |||
Thermal conductivity | 170.0 - 190.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 190.0 W/(m·K) | H12 | EN 573-3, EN 485 | ||
193 W/(m·K) Show Material materials with Thermal conductivity of 193 W/(m·K) | H12 | EN 573-3, EN 485 |
Electrical
Property | Value | Condition | Related Standards |
---|---|---|---|
Electrical conductivity | 23000000.0 - 26000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 26000000.0 S/m | H12 | EN 573-3, EN 485 |
29000000.0 S/m Show Material materials with Electrical conductivity of 29000000.0 S/m | H12 | EN 573-3, EN 485 | |
Electrical resistivity | 3.45e-08 Ω·m Show Material materials with Electrical resistivity of 3.45e-08 Ω·m | H12 | EN 573-3, EN 485 |
3.85e-08 - 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 3.85e-08 - 4.35e-08 Ω·m | H12 | EN 573-3, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | H12 | EN 573-3, EN 485 |
Copper | 0.05 % Show Material materials with Copper of 0.05 % | H12 | EN 573-3, EN 485 |
Iron | 0.45 % Show Material materials with Iron of 0.45 % | H12 | EN 573-3, EN 485 |
Magnesium | 1.1 - 1.7 % Show Material materials with Magnesium of 1.1 - 1.7 % | H12 | EN 573-3, EN 485 |
Manganese | 0.15 % Show Material materials with Manganese of 0.15 % | H12 | EN 573-3, EN 485 |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % | H12 | EN 573-3, EN 485 |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H12 | EN 573-3, EN 485 |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |