General
Property | Value | Condition | Related Standards |
---|---|---|---|
Density | 2.68 g/cm³ Show Material materials with Density of 2.68 g/cm³ | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Mechanical
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | H26 | EN 573-3, EN 485, EN 541, EN 754 | |
Bending angle 90° | 1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | H26 | EN 573-3, EN 485 | |
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | H26 | EN 573-3, EN 485 | ||
3.0 °/t Show Material materials with Bending angle 90° of 3.0 °/t | H26 | EN 573-3, EN 485 | ||
3.5 °/t Show Material materials with Bending angle 90° of 3.5 °/t | H26 | EN 573-3, EN 485 | ||
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H26 | EN 573-3, EN 485, EN 541, EN 754 | |
Hardness, Brinell | 74.0 [-] Show Material materials with Hardness, Brinell of 74.0 [-] | H26 | EN 573-3, EN 485 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Shear modulus | 26.3 GPa Show Material materials with Shear modulus of 26.3 GPa | H26 | EN 573-3, EN 485, EN 541, EN 754 | |
Tensile strength | 250.0 - 300.0 MPa Show Material materials with Tensile strength of 250.0 - 300.0 MPa | H26 | EN 573-3, EN 485 | |
250.0 - 290.0 MPa Show Material materials with Tensile strength of 250.0 - 290.0 MPa | H26 | EN 573-3, EN 754 | ||
260.0 - 300.0 MPa Show Material materials with Tensile strength of 260.0 - 300.0 MPa | H26 | EN 573-3, EN 541 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.2100000000000002e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2100000000000002e-05 1/K | H26 | EN 573-3, EN 485, EN 541, EN 754 | |
20 °C | 2.2100000000000002e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2100000000000002e-05 1/K | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
20 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
20 °C | 2.48e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.48e-05 1/K | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
20 °C | 2.5699999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5699999999999998e-05 1/K | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
100 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
200 °C | 2.48e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.48e-05 1/K | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
300 °C | 2.5699999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5699999999999998e-05 1/K | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Melting point | 605.0 - 650.0 °C Show Material materials with Melting point of 605.0 - 650.0 °C | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
607.0 - 649.0 °C Show Material materials with Melting point of 607.0 - 649.0 °C | H26 | EN 573-3, EN 485, EN 541, EN 754 | |||
Specific heat capacity | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
Thermal conductivity | 130.0 - 150.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 150.0 W/(m·K) | H26 | EN 573-3, EN 485, EN 541, EN 754 | ||
138 W/(m·K) Show Material materials with Thermal conductivity of 138 W/(m·K) | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Electrical
Property | Value | Condition | Related Standards |
---|---|---|---|
Electrical conductivity | 19000000.0 - 21000000.0 S/m Show Material materials with Electrical conductivity of 19000000.0 - 21000000.0 S/m | H26 | EN 573-3, EN 485, EN 541, EN 754 |
20000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 S/m | H26 | EN 573-3, EN 485, EN 541, EN 754 | |
Electrical resistivity | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with Electrical resistivity of 4.76e-08 - 5.26e-08 Ω·m | H26 | EN 573-3, EN 485, EN 541, EN 754 |
5e-08 Ω·m Show Material materials with Electrical resistivity of 5e-08 Ω·m | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Chromium | 0.15 - 0.35 % Show Material materials with Chromium of 0.15 - 0.35 % | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Iron | 0.40 % Show Material materials with Iron of 0.40 % | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Magnesium | 2.2 - 2.8 % Show Material materials with Magnesium of 2.2 - 2.8 % | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Manganese | 0.1 % Show Material materials with Manganese of 0.1 % | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Silicon | 0.25 % Show Material materials with Silicon of 0.25 % | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | H26 | EN 573-3, EN 485, EN 541, EN 754 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good, Protective: very good | |
Corrosion properties | Seawater: very good to good, weathering: good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |