General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.66 g/cm³ Show Material materials with Density of 2.66 g/cm³ | F | EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | ||
20.0 °C | 2.66 g/cm³ Show Material materials with Density of 2.66 g/cm³ | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Sheet, Strip, Tube |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 70.5 GPa Show Material materials with Elastic modulus of 70.5 GPa | F | EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | |||
20.0 °C | 68.0 - 72.0 GPa Show Material materials with Elastic modulus of 68.0 - 72.0 GPa | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Sheet, Strip, Tube | ||
Elongation | 12.0 % Show Material materials with Elongation of 12.0 % | F | EN 573-3, EN 755 | A50 | ||
14.0 % Show Material materials with Elongation of 14.0 % | F | EN 573-3, EN 755 | A100 | |||
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | Profile, Rod, Tube | A10 | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Tube | ||
20.0 °C | 23.0 % Show Material materials with Elongation of 23.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | |||
60.0 °C | 22.0 % Show Material materials with Elongation of 22.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | |||
100.0 °C | 21.0 % Show Material materials with Elongation of 21.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | |||
140.0 °C | 38.0 % Show Material materials with Elongation of 38.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | |||
180.0 °C | 38.0 % Show Material materials with Elongation of 38.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | |||
240.0 °C | 47.0 % Show Material materials with Elongation of 47.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | |||
300.0 °C | 66.0 % Show Material materials with Elongation of 66.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | |||
360.0 °C | 102.0 % Show Material materials with Elongation of 102.0 % | F | DIN 1725-1, EN 573-3, EN 573-4 | |||
Hardness, Brinell | 58.0 [-] Show Material materials with Hardness, Brinell of 58.0 [-] | F | EN 573-3, EN 570 | |||
20.0 °C | 45.0 [-] Show Material materials with Hardness, Brinell of 45.0 [-] | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Tube | ||
20.0 °C | 50.0 [-] Show Material materials with Hardness, Brinell of 50.0 [-] | F | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
20.0 °C | 60.0 [-] Show Material materials with Hardness, Brinell of 60.0 [-] | F | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Shear modulus | 26.5 GPa Show Material materials with Shear modulus of 26.5 GPa | F | EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | |||
20.0 °C | 27.0 GPa Show Material materials with Shear modulus of 27.0 GPa | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Sheet, Strip, Tube | ||
Tensile strength | 180.0 MPa Show Material materials with Tensile strength of 180.0 MPa | F | EN 573-3, EN 485, EN 755 | |||
190.0 - 250.0 MPa Show Material materials with Tensile strength of 190.0 - 250.0 MPa | F | EN 573-3, EN 1715-3, EN 1715-4 | ||||
190.0 MPa Show Material materials with Tensile strength of 190.0 MPa | F | EN 573-3, EN 485 | ||||
20.0 °C | 180.0 MPa Show Material materials with Tensile strength of 180.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Tube | ||
20.0 °C | 190.0 MPa Show Material materials with Tensile strength of 190.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
20.0 °C | 200.0 MPa Show Material materials with Tensile strength of 200.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4 | Sheet | ||
20.0 °C | 210.0 MPa Show Material materials with Tensile strength of 210.0 MPa | F | DIN 1725-1, EN 573-3, EN 573-4 | Sheet, Strip |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3899999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | ||
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3899999999999998e-05 1/K | F | EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | |||
100.0 °C | 2.39e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.39e-05 1/K | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Sheet, Strip, Tube | ||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Melting point | 610.0 - 640.0 °C Show Material materials with Melting point of 610.0 - 640.0 °C | F | EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | |||
Specific heat capacity | 20.0 °C | 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 963.0 J/(kg·K) | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Sheet, Strip, Tube | |
Thermal conductivity | 20.0 °C | 140.0 - 160.0 W/(m·K) Show Material materials with Thermal conductivity of 140.0 - 160.0 W/(m·K) | F | DIN 1725-1, EN 573-3, EN 573-4, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | Forging, Profile, Rod, Sheet, Strip, Tube |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 20000000.0 - 23000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 - 23000000.0 S/m | F | DIN 1725-1, EN 573-3, EN 573-4, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | Forging, Profile, Rod, Sheet, Strip, Tube |
Electrical resistivity | 4.35e-08 - 5e-08 Ω·m Show Material materials with Electrical resistivity of 4.35e-08 - 5e-08 Ω·m | F | EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.3 Show Material materials with Chromium of 0.3 | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Sheet, Strip, Tube |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | F | DIN 1725-1, EN 573-3, EN 573-4, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | Forging, Profile, Rod, Sheet, Strip, Tube |
Iron | 0.4 % Show Material materials with Iron of 0.4 % | F | DIN 1725-1, EN 573-3, EN 573-4 | Forging, Profile, Rod, Sheet, Strip, Tube |
0.40 % Show Material materials with Iron of 0.40 % | F | EN 573-3, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | ||
Magnesium | 2.6 - 3.6 % Show Material materials with Magnesium of 2.6 - 3.6 % | F | DIN 1725-1, EN 573-3, EN 573-4, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | Forging, Profile, Rod, Sheet, Strip, Tube |
Manganese | 0.5 % Show Material materials with Manganese of 0.5 % | F | DIN 1725-1, EN 573-3, EN 573-4, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | Forging, Profile, Rod, Sheet, Strip, Tube |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % | F | DIN 1725-1, EN 573-3, EN 573-4, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | Forging, Profile, Rod, Sheet, Strip, Tube |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | F | DIN 1725-1, EN 573-3, EN 573-4, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | Forging, Profile, Rod, Sheet, Strip, Tube |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | F | DIN 1725-1, EN 573-3, EN 573-4, EN 1386, EN 1715-3, EN 1715-4, EN 485, EN 570, EN 755 | Forging, Profile, Rod, Sheet, Strip, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good to good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |