DIN 1725-1 Grade 3.3527 F

Want to keep this datasheet? Save it now in your required format

Description

The alloy AlMg2Mn0,8 has similar characteristics as the alloy AlMg1,8. The additive of Mn (>0,6%) causes an increase of the heat resistance (up to 150°C) of the material and the recrystallisation limit. The result of the last is, that in case of extruded profiles the strength in longitudinal direction increases. The material is characterised by a good corrosion resistance. It is sea water steady and steady against saline atmosphere. With the Mg content the strength increases, the cold forming capacity decreases. The alloy is nature hard, i.e. that only by a cold forming shaping however by a purposeful heat treatment a strength increase cannot be attained. The splinter-giving workability and the weldability are improved with increasing Mg content. Application: In the apparatus engineering for receivers accordint to AD-W6/1 and according to VdTUEV-Werkstoffblaetter, for compressed gas tanks (pipings), for very low-temperature tanks and for temperatures to 250 °C. In the automobile engineering for utilizable superstructures, silo trucks, in shipbuilding for trunk and superstructures. In the building industry for roofings, claddings, for carrying constructions according to DIN 4173 and sun protection facilities as well as for furniture (including camping furniture).

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

F

EN 573-3, EN 485, EN 755

20.0 °C

2.71 g/cm³

Show Material materials with Density of 2.71 g/cm³

F

DIN 1725-1, EN 573-3, EN 573-4

Rod, Sheet, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

EN 573-3, EN 485, EN 755

20.0 °C

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

F

DIN 1725-1, EN 573-3, EN 573-4

Rod, Sheet, Tube

Elongation

13.0 %

Show Material materials with Elongation of 13.0 %

F

EN 573-3, EN 755

A50

15.0 %

Show Material materials with Elongation of 15.0 %

F

EN 573-3, EN 755

A100

20.0 °C

10.0 %

Show Material materials with Elongation of 10.0 %

F

DIN 1725-1, EN 573-3, EN 573-4

Sheet

20.0 °C

11.0 %

Show Material materials with Elongation of 11.0 %

F

DIN 1725-1, EN 573-3, EN 573-4

Rod, Tube

A10

20.0 °C

12.0 %

Show Material materials with Elongation of 12.0 %

F

DIN 1725-1, EN 573-3, EN 573-4

Sheet

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

F

DIN 1725-1, EN 573-3, EN 573-4

Rod, Tube

Hardness, Brinell

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

F

EN 573-3, EN 755

20.0 °C

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

F

DIN 1725-1, EN 573-3, EN 573-4

Rod, Sheet, Tube

20.0 °C

60.0 [-]

Show Material materials with Hardness, Brinell of 60.0 [-]

F

DIN 1725-1, EN 573-3, EN 573-4

Sheet

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

20.0 °C

26.5

Show Material materials with Shear modulus of 26.5

F

DIN 1725-1, EN 573-3, EN 573-4

Rod, Sheet, Tube

Tensile strength

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

F

EN 573-3, EN 755

190.0 MPa

Show Material materials with Tensile strength of 190.0 MPa

F

EN 573-3, EN 485

20.0 °C

190.0 - 230.0 MPa

Show Material materials with Tensile strength of 190.0 - 230.0 MPa

F

DIN 1725-1, EN 573-3, EN 573-4

Sheet

20.0 °C

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

F

DIN 1725-1, EN 573-3, EN 573-4

Rod, Tube

20.0 °C

200.0 - 240.0 MPa

Show Material materials with Tensile strength of 200.0 - 240.0 MPa

F

DIN 1725-1, EN 573-3, EN 573-4

Sheet

20.0 °C

210.0 - 250.0 MPa

Show Material materials with Tensile strength of 210.0 - 250.0 MPa

F

DIN 1725-1, EN 573-3, EN 573-4

Sheet

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

F

EN 573-3, EN 485, EN 755

100 °C

2.3699999999999997e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3699999999999997e-05 1/K

F

EN 573-3, EN 485, EN 755

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

F

DIN 1725-1, EN 573-3, EN 573-4

Rod, Sheet, Tube

Long

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

620.0 - 650.0 °C

Show Material materials with Melting point of 620.0 - 650.0 °C

F

EN 573-3, EN 485, EN 755

Specific heat capacity

879.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K)

Typical for Wrought 5000 Series Aluminium

Thermal conductivity

20.0 °C

140.0 - 180.0 W/(m·K)

Show Material materials with Thermal conductivity of 140.0 - 180.0 W/(m·K)

F

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 755

Rod, Sheet, Tube

Electrical

PropertyTemperatureValueConditionRelated StandardsShape

Electrical conductivity

20.0 °C

20000000.0 - 25000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 25000000.0 S/m

F

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 755

Rod, Sheet, Tube

Electrical resistivity

4e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 4e-08 - 5e-08 Ω·m

F

EN 573-3, EN 485, EN 755

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.3 %

Show Material materials with Chromium of 0.3 %

F

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 755

Rod, Sheet, Tube

Copper

0.1 %

Show Material materials with Copper of 0.1 %

F

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 755

Rod, Sheet, Tube

Iron

0.5 %

Show Material materials with Iron of 0.5 %

F

DIN 1725-1, EN 573-3, EN 573-4

Rod, Sheet, Tube

0.50 %

Show Material materials with Iron of 0.50 %

F

EN 573-3, EN 485, EN 755

Magnesium

1.6 - 2.5 %

Show Material materials with Magnesium of 1.6 - 2.5 %

F

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 755

Rod, Sheet, Tube

Manganese

0.5 - 1.1 %

Show Material materials with Manganese of 0.5 - 1.1 %

F

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 755

Rod, Sheet, Tube

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

F

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 755

Rod, Sheet, Tube

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

F

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 755

Rod, Sheet, Tube

Zinc

0.2 %

Show Material materials with Zinc of 0.2 %

F

DIN 1725-1, EN 573-3, EN 573-4, EN 485, EN 755

Rod, Sheet, Tube

Technological properties

Property
Anodizing

decorative: sufficient, Protective: good

Brazing

hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor

Corrosion properties

Seawater: very good, weathering: very good

Workability

Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12)