General
Property | Value | Condition | Related Standards |
---|---|---|---|
Density | 2.66 g/cm³ Show Material materials with Density of 2.66 g/cm³ | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Mechanical
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending angle 180° | 1.0 °/t Show Material materials with Bending angle 180° of 1.0 °/t | H111 | EN 573-3, EN 485 | |
1.5 °/t Show Material materials with Bending angle 180° of 1.5 °/t | H111 | EN 573-3, EN 14286, EN 485 | ||
3.0 °/t Show Material materials with Bending angle 180° of 3.0 °/t | H111 | EN 573-3, EN 14286 | ||
Bending angle 90° | 0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H111 | EN 573-3, EN 485 | |
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | ||
1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | H111 | EN 573-3, EN 485 | ||
2.5 °/t Show Material materials with Bending angle 90° of 2.5 °/t | H111 | EN 573-3, EN 485 | ||
Elastic modulus | 71.0 GPa Show Material materials with Elastic modulus of 71.0 GPa | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | |
Hardness, Brinell | 65.0 [-] Show Material materials with Hardness, Brinell of 65.0 [-] | H111 | EN 573-3, EN 485 | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||
Shear modulus | 26.7 GPa Show Material materials with Shear modulus of 26.7 GPa | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | |
Tensile strength | 240.0 - 310.0 MPa Show Material materials with Tensile strength of 240.0 - 310.0 MPa | H111 | EN 573-3, EN 14286, EN 485 | |
240.0 - 320.0 MPa Show Material materials with Tensile strength of 240.0 - 320.0 MPa | H111 | EN 573-3, EN 754, EN 755 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.2e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | |
20 °C | 2.2e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.2e-05 1/K | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
20 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
20 °C | 2.4699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
20 °C | 2.58e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
100 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
200 °C | 2.4699999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4699999999999997e-05 1/K | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
300 °C | 2.58e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.58e-05 1/K | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
Max service temperature | 150.0 °C Show Material materials with Max service temperature of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||
Melting point | 585.0 - 641.0 °C Show Material materials with Melting point of 585.0 - 641.0 °C | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
585.0 - 640.0 °C Show Material materials with Melting point of 585.0 - 640.0 °C | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | |||
Specific heat capacity | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
Thermal conductivity | 120.0 - 140.0 W/(m·K) Show Material materials with Thermal conductivity of 120.0 - 140.0 W/(m·K) | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | ||
126 W/(m·K) Show Material materials with Thermal conductivity of 126 W/(m·K) | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Electrical
Property | Value | Condition | Related Standards |
---|---|---|---|
Electrical conductivity | 17000000.0 - 19000000.0 S/m Show Material materials with Electrical conductivity of 17000000.0 - 19000000.0 S/m | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
18000000.0 S/m Show Material materials with Electrical conductivity of 18000000.0 S/m | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 | |
Electrical resistivity | 5.26e-08 - 5.88e-08 Ω·m Show Material materials with Electrical resistivity of 5.26e-08 - 5.88e-08 Ω·m | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
5.56e-08 Ω·m Show Material materials with Electrical resistivity of 5.56e-08 Ω·m | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Chromium | 0.05 - 0.25 % Show Material materials with Chromium of 0.05 - 0.25 % | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Iron | 0.50 % Show Material materials with Iron of 0.50 % | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Magnesium | 3.5 - 4.5 % Show Material materials with Magnesium of 3.5 - 4.5 % | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Manganese | 0.2 - 0.7 % Show Material materials with Manganese of 0.2 - 0.7 % | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Silicon | 0.4 % Show Material materials with Silicon of 0.4 % | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | H111 | EN 573-3, EN 14286, EN 485, EN 754, EN 755 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |