General
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 69.5 GPa Show Material materials with Elastic modulus of 69.5 GPa | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | |||
20.0 °C | 67.0 GPa Show Material materials with Elastic modulus of 67.0 GPa | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | Wire | ||
Elongation | 10.0 % Show Material materials with Elongation of 10.0 % | T4 | EN 573-3, EN 754 | A50 | ||
12.0 % Show Material materials with Elongation of 12.0 % | T4 | EN 573-3, EN 754 | A100 | |||
13.0 % Show Material materials with Elongation of 13.0 % | T4 | EN 573-3, EN 1301 | ||||
13.0 % Show Material materials with Elongation of 13.0 % | T4 | EN 573-3, EN 754 | A50 | |||
14.0 % Show Material materials with Elongation of 14.0 % | T4 | EN 573-3, EN 755 | A50 | |||
15.0 % Show Material materials with Elongation of 15.0 % | T4 | EN 573-3, EN 754 | A100 | |||
16.0 % Show Material materials with Elongation of 16.0 % | T4 | EN 573-3, EN 755 | A100 | |||
20.0 °C | 9.0 % Show Material materials with Elongation of 9.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | Wire | A100 | |
20.0 °C | 13.0 % Show Material materials with Elongation of 13.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | Wire | A10 | |
Hardness, Brinell | 20.0 °C | 45.0 [-] Show Material materials with Hardness, Brinell of 45.0 [-] | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | Wire | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Shear modulus | 26.1 GPa Show Material materials with Shear modulus of 26.1 GPa | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | |||
20.0 °C | 25.0 GPa Show Material materials with Shear modulus of 25.0 GPa | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | Wire | ||
Tensile strength | 120.0 MPa Show Material materials with Tensile strength of 120.0 MPa | T4 | EN 573-3, EN 755 | |||
130.0 MPa Show Material materials with Tensile strength of 130.0 MPa | T4 | EN 573-3, EN 754 | ||||
140.0 MPa Show Material materials with Tensile strength of 140.0 MPa | T4 | EN 573-3, EN 1301 | ||||
155.0 - 210.0 MPa Show Material materials with Tensile strength of 155.0 - 210.0 MPa | T4 | EN 573-3, EN 1715-3 | ||||
20.0 °C | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.18e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | |
20 °C | 2.18e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
20 °C | 2.45e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
20 °C | 2.56e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
200 °C | 2.45e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
300 °C | 2.56e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
Melting point | 585.0 - 650.0 °C Show Material materials with Melting point of 585.0 - 650.0 °C | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
Specific heat capacity | 898.0 J/(kg·K) Show Material materials with Specific heat capacity of 898.0 J/(kg·K) | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
Thermal conductivity | 200.0 - 220.0 W/(m·K) Show Material materials with Thermal conductivity of 200.0 - 220.0 W/(m·K) | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
20.0 °C | 220.0 W/(m·K) Show Material materials with Thermal conductivity of 220.0 W/(m·K) | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 34000000.0 - 38000000.0 S/m Show Material materials with Electrical conductivity of 34000000.0 - 38000000.0 S/m | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 | ||
20.0 °C | 30000000.0 - 32000000.0 S/m Show Material materials with Electrical conductivity of 30000000.0 - 32000000.0 S/m | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4 | Wire | |
Electrical resistivity | 2.63e-08 - 2.94e-08 Ω·m Show Material materials with Electrical resistivity of 2.63e-08 - 2.94e-08 Ω·m | T4 | EN 573-3, EN 1301, EN 1715-3, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.05 % Show Material materials with Chromium of 0.05 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 1301, EN 1715-3, EN 754, EN 755 | Wire |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 1301, EN 1715-3, EN 754, EN 755 | Wire |
Iron | 0.1 - 0.3 % Show Material materials with Iron of 0.1 - 0.3 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 1301, EN 1715-3, EN 754, EN 755 | Wire |
Magnesium | 0.35 - 0.6 % Show Material materials with Magnesium of 0.35 - 0.6 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 1301, EN 1715-3, EN 754, EN 755 | Wire |
Manganese | 0.1 % Show Material materials with Manganese of 0.1 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 1301, EN 1715-3, EN 754, EN 755 | Wire |
Silicon | 0.3 - 0.6 % Show Material materials with Silicon of 0.3 - 0.6 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 1301, EN 1715-3, EN 754, EN 755 | Wire |
Titanium | 0.1 % Show Material materials with Titanium of 0.1 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 1301, EN 1715-3, EN 754, EN 755 | Wire |
Zinc | 0.15 % Show Material materials with Zinc of 0.15 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 492, VdTÜV WB 420-4, EN 1301, EN 1715-3, EN 754, EN 755 | Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: EQ: sehr gut, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / good, friction soldering: very good, soft brazing with flux: good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / -, Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) - / good (O) |