General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | ||
20.0 °C | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 100.0 MPa Show Material materials with Bending Fatigue Strength of 100.0 MPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | |||
Bending angle 180° | 3.0 °/t Show Material materials with Bending angle 180° of 3.0 °/t | T4 | EN 573-3, EN 485 | |||
Bending angle 90° | 1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | T4 | EN 573-3, EN 485 | |||
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | T4 | EN 573-3, EN 485 | ||||
3.0 °/t Show Material materials with Bending angle 90° of 3.0 °/t | T4 | EN 573-3, EN 485 | ||||
4.0 °/t Show Material materials with Bending angle 90° of 4.0 °/t | T4 | EN 573-3, EN 1386, EN 485 | ||||
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | |||
20.0 °C | 68.0 - 73.0 GPa Show Material materials with Elastic modulus of 68.0 - 73.0 GPa | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire | ||
Elongation | 6.0 % Show Material materials with Elongation of 6.0 % | T4 | EN 573-3, EN 1386 | A50 | ||
8.0 % Show Material materials with Elongation of 8.0 % | T4 | EN 573-3, EN 1386 | A50 | |||
10.0 % Show Material materials with Elongation of 10.0 % | T4 | EN 573-3, EN 1386 | A50 | |||
12.0 % Show Material materials with Elongation of 12.0 % | T4 | EN 573-3, EN 1386 | A100 | |||
12.0 % Show Material materials with Elongation of 12.0 % | T4 | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | A50 | |||
13.0 % Show Material materials with Elongation of 13.0 % | T4 | EN 573-3, EN 1301 | ||||
14.0 % Show Material materials with Elongation of 14.0 % | T4 | EN 573-3, EN 754, EN 755 | A100 | |||
14.0 % Show Material materials with Elongation of 14.0 % | T4 | EN 573-3, EN 485 | A50 | |||
15.0 % Show Material materials with Elongation of 15.0 % | T4 | EN 573-3, EN 485 | A50 | |||
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | A100 | |
20.0 °C | 11.0 % Show Material materials with Elongation of 11.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Wire | A10 | |
20.0 °C | 12.0 % Show Material materials with Elongation of 12.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | ||
Hardness, Brinell | 58.0 [-] Show Material materials with Hardness, Brinell of 58.0 [-] | T4 | EN 573-3, EN 485 | |||
20.0 °C | 60.0 [-] Show Material materials with Hardness, Brinell of 60.0 [-] | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire | ||
20.0 °C | 65.0 [-] Show Material materials with Hardness, Brinell of 65.0 [-] | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Shear modulus | 26.4 GPa Show Material materials with Shear modulus of 26.4 GPa | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | |||
20.0 °C | 26.0 - 27.0 GPa Show Material materials with Shear modulus of 26.0 - 27.0 GPa | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire | ||
Tensile strength | 205.0 MPa Show Material materials with Tensile strength of 205.0 MPa | T4 | EN 573-3, EN 1301, EN 1386, EN 485, EN 754, EN 755 | |||
260.0 - 290.0 MPa Show Material materials with Tensile strength of 260.0 - 290.0 MPa | T4 | EN 573-3, EN 1715-3 | ||||
20.0 °C | 200.0 MPa Show Material materials with Tensile strength of 200.0 MPa | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | ||
Melting point | 585.0 - 650.0 °C Show Material materials with Melting point of 585.0 - 650.0 °C | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | ||
Specific heat capacity | 896.0 J/(kg·K) Show Material materials with Specific heat capacity of 896.0 J/(kg·K) | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | ||
Thermal conductivity | 20.0 °C | 170.0 - 220.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 220.0 W/(m·K) | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Forging, Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 20.0 °C | 24000000.0 - 32000000.0 S/m Show Material materials with Electrical conductivity of 24000000.0 - 32000000.0 S/m | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Forging, Wire |
Electrical resistivity | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with Electrical resistivity of 3.13e-08 - 4.17e-08 Ω·m | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.25 % Show Material materials with Chromium of 0.25 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Forging, Wire |
Copper | 0.1 % Show Material materials with Copper of 0.1 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Forging, Wire |
Iron | 0.5 % Show Material materials with Iron of 0.5 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493 | Forging, Wire |
0.50 % Show Material materials with Iron of 0.50 % | T4 | EN 573-3, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | ||
Magnesium | 0.6 - 1.2 % Show Material materials with Magnesium of 0.6 - 1.2 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Forging, Wire |
Manganese | 0.4 - 1.0 % Show Material materials with Manganese of 0.4 - 1.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Forging, Wire |
Silicon | 0.7 - 1.3 % Show Material materials with Silicon of 0.7 - 1.3 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Forging, Wire |
Titanium | 0.1 % Show Material materials with Titanium of 0.1 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Forging, Wire |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, VdTÜV WB 240, VdTÜV WB 414, VdTÜV WB 327, VdTÜV WB 423, VdTÜV WB 493, EN 1301, EN 1386, EN 1715-3, EN 485, EN 754, EN 755 | Forging, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |