General
Property | Value | Condition | Related Standards |
---|---|---|---|
Density | 2.7 g/cm³ Show Material materials with Density of 2.7 g/cm³ | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Mechanical
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 95.0 MPa Show Material materials with Bending Fatigue Strength of 95.0 MPa | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 754, EN 755 | |
Bending angle 90° | 2.5 °/t Show Material materials with Bending angle 90° of 2.5 °/t | T6 | EN 573-3, EN 485 | |
3.5 °/t Show Material materials with Bending angle 90° of 3.5 °/t | T6 | EN 573-3, EN 485 | ||
4.0 °/t Show Material materials with Bending angle 90° of 4.0 °/t | T6 | EN 573-3, EN 485 | ||
5.0 °/t Show Material materials with Bending angle 90° of 5.0 °/t | T6 | EN 573-3, EN 485 | ||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | |
70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | ||
Elongation | 2.0 % Show Material materials with Elongation of 2.0 % | T6 | EN 573-3, EN 485 | A100 |
3.0 % Show Material materials with Elongation of 3.0 % | T6 | EN 573-3, EN 1386 | A50 | |
4.0 % Show Material materials with Elongation of 4.0 % | T6 | EN 573-3, EN 1386 | A50 | |
4.0 % Show Material materials with Elongation of 4.0 % | T6 | EN 573-3, EN 485 | A100 | |
5.0 % Show Material materials with Elongation of 5.0 % | T6 | EN 573-3, EN 13981-1, EN 485 | A100 | |
6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3, EN 1386, EN 485, EN 755 | A50 | |
6.0 % Show Material materials with Elongation of 6.0 % | T6 | EN 573-3, EN 485 | A100 | |
7.0 % Show Material materials with Elongation of 7.0 % | T6 | EN 573-3, EN 485, EN 755 | A50 | |
8.0 % Show Material materials with Elongation of 8.0 % | T6 | EN 573-3, EN 1386, EN 754, EN 755 | A50 | |
8.0 % Show Material materials with Elongation of 8.0 % | T6 | EN 573-3, EN 1386, EN 485, EN 755 | A100 | |
9.0 % Show Material materials with Elongation of 9.0 % | T6 | EN 573-3, EN 485 | A50 | |
9.0 % Show Material materials with Elongation of 9.0 % | T6 | EN 573-3, EN 755 | A100 | |
10.0 % Show Material materials with Elongation of 10.0 % | T6 | EN 573-3, EN 1301 | ||
10.0 % Show Material materials with Elongation of 10.0 % | T6 | EN 573-3, EN 485 | A50 | |
10.0 % Show Material materials with Elongation of 10.0 % | T6 | EN 573-3, EN 754, EN 755 | A100 | |
Hardness, Brinell | 80.0 [-] Show Material materials with Hardness, Brinell of 80.0 [-] | T6 | EN 573-3, EN 485 | |
81.0 [-] Show Material materials with Hardness, Brinell of 81.0 [-] | T6 | EN 573-3, EN 485 | ||
84.0 [-] Show Material materials with Hardness, Brinell of 84.0 [-] | T6 | EN 573-3, EN 485 | ||
85.0 [-] Show Material materials with Hardness, Brinell of 85.0 [-] | T6 | EN 573-3, EN 13981-1 | ||
88.0 [-] Show Material materials with Hardness, Brinell of 88.0 [-] | T6 | EN 573-3, EN 485 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Shear modulus | 26.3 GPa Show Material materials with Shear modulus of 26.3 GPa | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | |
Tensile strength | 260.0 MPa Show Material materials with Tensile strength of 260.0 MPa | T6 | EN 573-3, EN 13981-1, EN 485, EN 755 | |
265.0 MPa Show Material materials with Tensile strength of 265.0 MPa | T6 | EN 573-3, EN 485 | ||
275.0 MPa Show Material materials with Tensile strength of 275.0 MPa | T6 | EN 573-3, EN 485 | ||
290.0 MPa Show Material materials with Tensile strength of 290.0 MPa | T6 | EN 573-3, EN 1301, EN 1386, EN 485, EN 754 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | |
20 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | ||
100 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | ||
100 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | ||
Melting point | 580.0 - 640.0 °C Show Material materials with Melting point of 580.0 - 640.0 °C | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | ||
580.0 - 650.0 °C Show Material materials with Melting point of 580.0 - 650.0 °C | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | |||
Specific heat capacity | 887.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | |||
Thermal conductivity | 155.0 - 180.0 W/(m·K) Show Material materials with Thermal conductivity of 155.0 - 180.0 W/(m·K) | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | ||
170.0 - 200.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 200.0 W/(m·K) | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Electrical
Property | Value | Condition | Related Standards |
---|---|---|---|
Electrical conductivity | 22000000.0 - 30000000.0 S/m Show Material materials with Electrical conductivity of 22000000.0 - 30000000.0 S/m | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
23000000.0 - 27000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 27000000.0 S/m | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 | |
Electrical resistivity | 3.33e-08 - 4.55e-08 Ω·m Show Material materials with Electrical resistivity of 3.33e-08 - 4.55e-08 Ω·m | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
3.7e-08 - 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 3.7e-08 - 4.35e-08 Ω·m | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Chromium | 0.04 - 0.35 % Show Material materials with Chromium of 0.04 - 0.35 % | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Copper | 0.15 - 0.4 % Show Material materials with Copper of 0.15 - 0.4 % | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Iron | 0.70 % Show Material materials with Iron of 0.70 % | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Manganese | 0.15 % Show Material materials with Manganese of 0.15 % | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Silicon | 0.4 - 0.8 % Show Material materials with Silicon of 0.4 - 0.8 % | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T6 | EN 573-3, EN 1301, EN 1386, EN 13981-1, EN 485, EN 754, EN 755 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good to acceptable, weathering: good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |