General
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 MPa | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
Bending angle 180° | 1.0 °/t Show Material materials with Bending angle 180° of 1.0 °/t | O | EN 573-3, EN 485 | |||
Bending angle 90° | 0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | O | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | O | EN 573-3, EN 485 | ||||
2.0 °/t Show Material materials with Bending angle 90° of 2.0 °/t | O | EN 573-3, EN 1386, EN 485 | ||||
Elastic modulus | 69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||||
20.0 °C | 68.3 - 69.6 GPa Show Material materials with Elastic modulus of 68.3 - 69.6 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Strip | ||
Elongation | 6.0 % Show Material materials with Elongation of 6.0 % | O | EN 573-3, EN 1386 | A50 | ||
8.0 % Show Material materials with Elongation of 8.0 % | O | EN 573-3, EN 1386 | A50 | |||
10.0 % Show Material materials with Elongation of 10.0 % | O | EN 573-3, EN 1386 | A50 | |||
12.0 % Show Material materials with Elongation of 12.0 % | O | EN 573-3, EN 1386 | A50 | |||
13.0 % Show Material materials with Elongation of 13.0 % | O | EN 573-3, EN 1386 | A100 | |||
14.0 % Show Material materials with Elongation of 14.0 % | O | EN 573-3, EN 485, EN 754, EN 755 | A50 | |||
16.0 % Show Material materials with Elongation of 16.0 % | O | EN 573-3, EN 485 | A50 | |||
16.0 % Show Material materials with Elongation of 16.0 % | O | EN 573-3, EN 485, EN 754, EN 755 | A100 | |||
19.0 % Show Material materials with Elongation of 19.0 % | O | EN 573-3, EN 485 | A50 | |||
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet | A10 | |
20.0 °C | 14.0 % Show Material materials with Elongation of 14.0 % | O | WL 3.3214-1, DIN 1725-1 | Sheet | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Elongation of 15.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Strip, Sheet | A10 | |
20.0 °C | 15.0 % Show Material materials with Elongation of 15.0 % | O | WL 3.3214-1, DIN 1725-1 | Tube | A50 | |
20.0 °C | 16.0 % Show Material materials with Elongation of 16.0 % | O | WL 3.3214-1, DIN 1725-1 | Sheet | A50 Transverse | |
20.0 °C | 17.0 % Show Material materials with Elongation of 17.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet | ||
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Strip, Sheet | ||
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | O | WL 3.3214-1, DIN 1725-1 | Sheet | A50 Transverse | |
20.0 °C | 18.0 % Show Material materials with Elongation of 18.0 % | O | WL 3.3214-1, DIN 1725-1 | Sheet | Transverse | |
Hardness, Brinell | 40.0 [-] Show Material materials with Hardness, Brinell of 40.0 [-] | O | EN 573-3, EN 485 | |||
20.0 °C | 40.0 [-] Show Material materials with Hardness, Brinell of 40.0 [-] | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Strip, Sheet, Tube | ||
20.0 °C | 40.0 [-] Show Material materials with Hardness, Brinell of 40.0 [-] | O | WL 3.3214-1, DIN 1725-1 | Sheet | Transverse | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Shear modulus | 26.3 GPa Show Material materials with Shear modulus of 26.3 GPa | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
20.0 °C | 26.2 GPa Show Material materials with Shear modulus of 26.2 GPa | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Strip | ||
Tensile strength | 150.0 Show Material materials with Tensile strength of 150.0 | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
20.0 °C | 150.0 Show Material materials with Tensile strength of 150.0 | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Strip, Sheet, Tube | ||
20.0 °C | 150.0 MPa Show Material materials with Tensile strength of 150.0 MPa | O | WL 3.3214-1, DIN 1725-1 | Sheet | Transverse |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |
20 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
100 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
100 °C | 2.36e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
Melting point | 580.0 - 640.0 °C Show Material materials with Melting point of 580.0 - 640.0 °C | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
580.0 - 650.0 °C Show Material materials with Melting point of 580.0 - 650.0 °C | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
Specific heat capacity | 20.0 °C | 870.0 J/(kg·K) Show Material materials with Specific heat capacity of 870.0 J/(kg·K) | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Strip |
Thermal conductivity | 155.0 - 180.0 W/(m·K) Show Material materials with Thermal conductivity of 155.0 - 180.0 W/(m·K) | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
170.0 - 200.0 W/(m·K) Show Material materials with Thermal conductivity of 170.0 - 200.0 W/(m·K) | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
20.0 °C | 150.0 - 165.0 W/(m·K) Show Material materials with Thermal conductivity of 150.0 - 165.0 W/(m·K) | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Strip |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 22000000.0 - 30000000.0 S/m Show Material materials with Electrical conductivity of 22000000.0 - 30000000.0 S/m | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
23000000.0 - 27000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 - 27000000.0 S/m | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | |||
20.0 °C | 20000000.0 - 30000000.0 S/m Show Material materials with Electrical conductivity of 20000000.0 - 30000000.0 S/m | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Strip | |
Electrical resistivity | 3.33e-08 - 4.55e-08 Ω·m Show Material materials with Electrical resistivity of 3.33e-08 - 4.55e-08 Ω·m | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
3.7e-08 - 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 3.7e-08 - 4.35e-08 Ω·m | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.04 - 0.35 % Show Material materials with Chromium of 0.04 - 0.35 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Tube |
Copper | 0.15 - 0.4 % Show Material materials with Copper of 0.15 - 0.4 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Tube |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1 | Sheet, Strip, Tube |
0.70 % Show Material materials with Iron of 0.70 % | O | EN 573-3, EN 1386, EN 485, EN 754, EN 755 | ||
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Tube |
Manganese | 0.15 % Show Material materials with Manganese of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Tube |
Silicon | 0.4 - 0.8 % Show Material materials with Silicon of 0.4 - 0.8 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Tube |
Titanium | 0.15 % Show Material materials with Titanium of 0.15 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Tube |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | O | DIN 1725-1, EN 573-3, EN 573-4, WL 3.3214-1, EN 1386, EN 485, EN 754, EN 755 | Sheet, Strip, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good to acceptable, weathering: good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |