General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Density | 2.75 g/cm³ Show Material materials with Density of 2.75 g/cm³ | T4 | EN 573-3, EN 1301 | ||
20.0 °C | 2.74 g/cm³ Show Material materials with Density of 2.74 g/cm³ | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | |
20.0 °C | 2.75 g/cm³ Show Material materials with Density of 2.75 g/cm³ | T4 | WL 3.1124-1, DIN 1725-1 | Wire |
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | T4 | EN 573-3, EN 1301 | |||
20.0 °C | 67.0 GPa Show Material materials with Elastic modulus of 67.0 GPa | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | ||
20.0 °C | 71.1 GPa Show Material materials with Elastic modulus of 71.1 GPa | T4 | WL 3.1124-1, DIN 1725-1 | Wire | ||
Elongation | 20.0 % Show Material materials with Elongation of 20.0 % | T4 | EN 573-3, EN 1301 | |||
20.0 °C | 5.0 % Show Material materials with Elongation of 5.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | A100 | |
20.0 °C | 10.0 % Show Material materials with Elongation of 10.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | A10 | |
Hardness, Brinell | 20.0 °C | 75.0 [-] Show Material materials with Hardness, Brinell of 75.0 [-] | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Shear modulus | 20.0 °C | 25.5 GPa Show Material materials with Shear modulus of 25.5 GPa | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | |
Shear strength | 20.0 °C | 195.0 MPa Show Material materials with Shear strength of 195.0 MPa | T4 | WL 3.1124-1, DIN 1725-1 | Wire | |
Tensile strength | 260.0 MPa Show Material materials with Tensile strength of 260.0 MPa | T4 | EN 573-3, EN 1301 | |||
20.0 °C | 270.0 MPa Show Material materials with Tensile strength of 270.0 MPa | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50.0 °C | 2.18e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.18e-05 1/K | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire |
20 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | T4 | EN 573-3, EN 1301 | ||
100.0 °C | 2.34e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.34e-05 1/K | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | |
100 °C | 2.38e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K | T4 | EN 573-3, EN 1301 | ||
200.0 °C | 2.45e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.45e-05 1/K | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | |
300.0 °C | 2.56e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.56e-05 1/K | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | |
Melting point | 550.0 - 650.0 °C Show Material materials with Melting point of 550.0 - 650.0 °C | T4 | EN 573-3, EN 1301 | ||
Specific heat capacity | 20.0 °C | 898.0 J/(kg·K) Show Material materials with Specific heat capacity of 898.0 J/(kg·K) | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire |
20.0 °C | 920.0 J/(kg·K) Show Material materials with Specific heat capacity of 920.0 J/(kg·K) | T4 | WL 3.1124-1, DIN 1725-1 | Wire | |
Thermal conductivity | 155 W/(m·K) Show Material materials with Thermal conductivity of 155 W/(m·K) | T4 | EN 573-3, EN 1301 | ||
20.0 °C | 150.0 - 180.0 W/(m·K) Show Material materials with Thermal conductivity of 150.0 - 180.0 W/(m·K) | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 23000000.0 S/m Show Material materials with Electrical conductivity of 23000000.0 S/m | T4 | EN 573-3, EN 1301 | ||
20.0 °C | 21000000.0 - 25000000.0 S/m Show Material materials with Electrical conductivity of 21000000.0 - 25000000.0 S/m | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire | |
Electrical resistivity | 4.35e-08 Ω·m Show Material materials with Electrical resistivity of 4.35e-08 Ω·m | T4 | EN 573-3, EN 1301 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1, EN 1301 | Wire |
Copper | 2.2 - 3.0 % Show Material materials with Copper of 2.2 - 3.0 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1, EN 1301 | Wire |
Iron | 0.7 % Show Material materials with Iron of 0.7 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1 | Wire |
0.70 % Show Material materials with Iron of 0.70 % | T4 | EN 573-3, EN 1301 | ||
Magnesium | 0.2 - 0.5 % Show Material materials with Magnesium of 0.2 - 0.5 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1, EN 1301 | Wire |
Manganese | 0.2 % Show Material materials with Manganese of 0.2 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1, EN 1301 | Wire |
Silicon | 0.8 % Show Material materials with Silicon of 0.8 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1, EN 1301 | Wire |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T4 | DIN 1725-1, EN 573-3, EN 573-4, WL 3.1124-1, EN 1301 | Wire |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |