General
Property | Value | Condition | Related Standards |
---|---|---|---|
Density | 2.8 g/cm³ Show Material materials with Density of 2.8 g/cm³ | T451 | EN 573-3, EN 485 |
Mechanical
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending angle 180° | 3.0 °/t Show Material materials with Bending angle 180° of 3.0 °/t | T451 | EN 573-3, EN 485 | |
5.0 °/t Show Material materials with Bending angle 180° of 5.0 °/t | T451 | EN 573-3, EN 485 | ||
Bending angle 90° | 3.0 °/t Show Material materials with Bending angle 90° of 3.0 °/t | T451 | EN 573-3, EN 485 | |
5.0 °/t Show Material materials with Bending angle 90° of 5.0 °/t | T451 | EN 573-3, EN 485 | ||
8.0 °/t Show Material materials with Bending angle 90° of 8.0 °/t | T451 | EN 573-3, EN 485 | ||
Elastic modulus | 72.5 GPa Show Material materials with Elastic modulus of 72.5 GPa | T451 | EN 573-3, EN 485 | |
Hardness, Brinell | 101.0 [-] Show Material materials with Hardness, Brinell of 101.0 [-] | T451 | EN 573-3, EN 485 | |
105.0 [-] Show Material materials with Hardness, Brinell of 105.0 [-] | T451 | EN 573-3, EN 485 | ||
108.0 [-] Show Material materials with Hardness, Brinell of 108.0 [-] | T451 | EN 573-3, EN 485 | ||
110.0 [-] Show Material materials with Hardness, Brinell of 110.0 [-] | T451 | EN 573-3, EN 485 | ||
111.0 [-] Show Material materials with Hardness, Brinell of 111.0 [-] | T451 | EN 573-3, EN 485 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Shear modulus | 27.2 GPa Show Material materials with Shear modulus of 27.2 GPa | T451 | EN 573-3, EN 485 | |
Tensile strength | 300.0 MPa Show Material materials with Tensile strength of 300.0 MPa | T451 | EN 573-3, EN 485 | |
330.0 MPa Show Material materials with Tensile strength of 330.0 MPa | T451 | EN 573-3, EN 485 | ||
350.0 MPa Show Material materials with Tensile strength of 350.0 MPa | T451 | EN 573-3, EN 485 | ||
360.0 MPa Show Material materials with Tensile strength of 360.0 MPa | T451 | EN 573-3, EN 485 | ||
370.0 MPa Show Material materials with Tensile strength of 370.0 MPa | T451 | EN 573-3, EN 485 | ||
385.0 MPa Show Material materials with Tensile strength of 385.0 MPa | T451 | EN 573-3, EN 485 | ||
390.0 MPa Show Material materials with Tensile strength of 390.0 MPa | T451 | EN 573-3, EN 485 |
Thermal
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 20 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | T451 | EN 573-3, EN 485 | |
100 °C | 2.3e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K | T451 | EN 573-3, EN 485 | ||
Melting point | 512.0 - 650.0 °C Show Material materials with Melting point of 512.0 - 650.0 °C | T451 | EN 573-3, EN 485 | ||
Specific heat capacity | 816.0 - 963.0 J/(kg·K) Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | |||
Thermal conductivity | 130.0 - 200.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 200.0 W/(m·K) | T451 | EN 573-3, EN 485 |
Electrical
Property | Value | Condition | Related Standards |
---|---|---|---|
Electrical conductivity | 18000000.0 - 28000000.0 S/m Show Material materials with Electrical conductivity of 18000000.0 - 28000000.0 S/m | T451 | EN 573-3, EN 485 |
Electrical resistivity | 3.57e-08 - 5.56e-08 Ω·m Show Material materials with Electrical resistivity of 3.57e-08 - 5.56e-08 Ω·m | T451 | EN 573-3, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Chromium | 0.1 % Show Material materials with Chromium of 0.1 % | T451 | EN 573-3, EN 485 |
Copper | 3.5 - 4.5 % Show Material materials with Copper of 3.5 - 4.5 % | T451 | EN 573-3, EN 485 |
Iron | 0.70 % Show Material materials with Iron of 0.70 % | T451 | EN 573-3, EN 485 |
Magnesium | 0.4 - 1.0 % Show Material materials with Magnesium of 0.4 - 1.0 % | T451 | EN 573-3, EN 485 |
Manganese | 0.4 - 1.0 % Show Material materials with Manganese of 0.4 - 1.0 % | T451 | EN 573-3, EN 485 |
Silicon | 0.2 - 0.8 % Show Material materials with Silicon of 0.2 - 0.8 % | T451 | EN 573-3, EN 485 |
Zinc | 0.25 % Show Material materials with Zinc of 0.25 % | T451 | EN 573-3, EN 485 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: poor, weathering: sufficient | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) acceptable (O) / acceptable (O) |