Property | Value | Condition | Related Standards |
---|---|---|---|
Density | 2.77 g/cm³ Show Material materials with Density of 2.77 g/cm³ | T62 | EN 573-3, EN 485 |
Mechanical
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending angle 90° | 3.5 °/t Show Material materials with Bending angle 90° of 3.5 °/t | T62 | EN 573-3, EN 485 | |
4.0 °/t Show Material materials with Bending angle 90° of 4.0 °/t | T62 | EN 573-3, EN 485 | ||
5.5 °/t Show Material materials with Bending angle 90° of 5.5 °/t | T62 | EN 573-3, EN 485 | ||
8.0 °/t Show Material materials with Bending angle 90° of 8.0 °/t | T62 | EN 573-3, EN 485 | ||
Elastic modulus | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | T62 | EN 573-3, EN 485 | |
Hardness, Brinell | 98.0 [-] Show Material materials with Hardness, Brinell of 98.0 [-] | T62 | EN 573-3, EN 485 | |
101.0 [-] Show Material materials with Hardness, Brinell of 101.0 [-] | T62 | EN 573-3, EN 485 | ||
104.0 [-] Show Material materials with Hardness, Brinell of 104.0 [-] | T62 | EN 573-3, EN 485 | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||
Shear modulus | 26.4 GPa Show Material materials with Shear modulus of 26.4 GPa | T62 | EN 573-3, EN 485 | |
Tensile strength | 330.0 MPa Show Material materials with Tensile strength of 330.0 MPa | T62 | EN 573-3, EN 485 | |
340.0 MPa Show Material materials with Tensile strength of 340.0 MPa | T62 | EN 573-3, EN 485 | ||
350.0 MPa Show Material materials with Tensile strength of 350.0 MPa | T62 | EN 573-3, EN 485 |
Thermal
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.14e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K | T62 | EN 573-3, EN 485 |
20 °C | 2.14e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.14e-05 1/K | T62 | EN 573-3, EN 485 | |
20 °C | 2.31e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.31e-05 1/K | T62 | EN 573-3, EN 485 | |
20 °C | 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K | T62 | EN 573-3, EN 485 | |
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K | T62 | EN 573-3, EN 485 | |
100 °C | 2.31e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.31e-05 1/K | T62 | EN 573-3, EN 485 | |
200 °C | 2.4e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4e-05 1/K | T62 | EN 573-3, EN 485 | |
300 °C | 2.4999999999999998e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4999999999999998e-05 1/K | T62 | EN 573-3, EN 485 | |
Melting point | 600.0 - 650.0 °C Show Material materials with Melting point of 600.0 - 650.0 °C | T62 | EN 573-3, EN 485 | |
Specific heat capacity | 875.0 J/(kg·K) Show Material materials with Specific heat capacity of 875.0 J/(kg·K) | T62 | EN 573-3, EN 485 | |
Thermal conductivity | 130.0 - 160.0 W/(m·K) Show Material materials with Thermal conductivity of 130.0 - 160.0 W/(m·K) | T62 | EN 573-3, EN 485 |
Electrical
Property | Value | Condition | Related Standards |
---|---|---|---|
Electrical conductivity | 19000000.0 - 23000000.0 S/m Show Material materials with Electrical conductivity of 19000000.0 - 23000000.0 S/m | T62 | EN 573-3, EN 485 |
Electrical resistivity | 4.35e-08 - 5.26e-08 Ω·m Show Material materials with Electrical resistivity of 4.35e-08 - 5.26e-08 Ω·m | T62 | EN 573-3, EN 485 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Copper | 0.2 % Show Material materials with Copper of 0.2 % | T62 | EN 573-3, EN 485 |
Iron | 0.40 % Show Material materials with Iron of 0.40 % | T62 | EN 573-3, EN 485 |
Magnesium | 1.0 - 1.4 % Show Material materials with Magnesium of 1.0 - 1.4 % | T62 | EN 573-3, EN 485 |
Manganese | 0.05 - 0.5 % Show Material materials with Manganese of 0.05 - 0.5 % | T62 | EN 573-3, EN 485 |
Silicon | 0.35 % Show Material materials with Silicon of 0.35 % | T62 | EN 573-3, EN 485 |
Zinc | 4.0 - 5.0 % Show Material materials with Zinc of 4.0 - 5.0 % | T62 | EN 573-3, EN 485 |
Zirconium | 0.08 - 0.2 % Show Material materials with Zirconium of 0.08 - 0.2 % | T62 | EN 573-3, EN 485 |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): good (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) good (O) / good (O) |