EN 573-3 Grade 3.4365 T62

Want to keep this datasheet? Save it now in your required format

Description

DIN 3.4365 is a high-strength alloy that offers good stress-corrosion cracking resistance. Known as a mainstay in the aerospace industry since it was introduced, Aluminum 7075 brings moderate toughness as well as an excellent strength-to-weight ratio. It is also important to note that at sub-zero temperatures Aluminum 7075 increases in strength.

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T62

EN 573-3, EN 485, EN 603

Mechanical

PropertyValueConditionRelated StandardsComment

Bending angle 90°

12.0 °/t

Show Material materials with Bending angle 90° of 12.0 °/t

T62

EN 573-3, EN 485

4.5 °/t

Show Material materials with Bending angle 90° of 4.5 °/t

T62

EN 573-3, EN 485

5.5 °/t

Show Material materials with Bending angle 90° of 5.5 °/t

T62

EN 573-3, EN 485

6.5 °/t

Show Material materials with Bending angle 90° of 6.5 °/t

T62

EN 573-3, EN 485

8.0 °/t

Show Material materials with Bending angle 90° of 8.0 °/t

T62

EN 573-3, EN 485

Elastic modulus

72.0 GPa

Show Material materials with Elastic modulus of 72.0 GPa

T62

EN 573-3, EN 485, EN 603

Hardness, Brinell

160.0 [-]

Show Material materials with Hardness, Brinell of 160.0 [-]

T62

EN 573-3, EN 485

158.0 [-]

Show Material materials with Hardness, Brinell of 158.0 [-]

T62

EN 573-3, EN 485

157.0 [-]

Show Material materials with Hardness, Brinell of 157.0 [-]

T62

EN 573-3, EN 485

155.0 [-]

Show Material materials with Hardness, Brinell of 155.0 [-]

T62

EN 573-3, EN 485

144.0 [-]

Show Material materials with Hardness, Brinell of 144.0 [-]

T62

EN 573-3, EN 485

119.0 [-]

Show Material materials with Hardness, Brinell of 119.0 [-]

T62

EN 573-3, EN 485

161.0 [-]

Show Material materials with Hardness, Brinell of 161.0 [-]

T62

EN 573-3, EN 485

147.0 [-]

Show Material materials with Hardness, Brinell of 147.0 [-]

T62

EN 573-3, EN 485

104.0 [-]

Show Material materials with Hardness, Brinell of 104.0 [-]

T62

EN 573-3, EN 485

135.0 [-]

Show Material materials with Hardness, Brinell of 135.0 [-]

T62

EN 573-3, EN 485

163.0 [-]

Show Material materials with Hardness, Brinell of 163.0 [-]

T62

EN 573-3, EN 485

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 7000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 7000 Series Aluminium

Shear modulus

27.1 GPa

Show Material materials with Shear modulus of 27.1 GPa

T62

EN 573-3, EN 485, EN 603

Tensile strength

360.0 MPa

Show Material materials with Tensile strength of 360.0 MPa

T62

EN 573-3, EN 485

540.0 MPa

Show Material materials with Tensile strength of 540.0 MPa

T62

EN 573-3, EN 485

530.0 MPa

Show Material materials with Tensile strength of 530.0 MPa

T62

EN 573-3, EN 485

525.0 MPa

Show Material materials with Tensile strength of 525.0 MPa

T62

EN 573-3, EN 485

490.0 MPa

Show Material materials with Tensile strength of 490.0 MPa

T62

EN 573-3, EN 485

410.0 MPa

Show Material materials with Tensile strength of 410.0 MPa

T62

EN 573-3, EN 485

495.0 MPa

Show Material materials with Tensile strength of 495.0 MPa

T62

EN 573-3, EN 485

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T62

EN 573-3, EN 485

545.0 MPa

Show Material materials with Tensile strength of 545.0 MPa

T62

EN 573-3, EN 485

510.0 MPa

Show Material materials with Tensile strength of 510.0 MPa

T62

EN 573-3, EN 603

Thermal

PropertyTemperatureValueConditionRelated Standards

Coefficient of thermal expansion

300 °C, 20 °C

2.52e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.52e-05 1/K

T62

EN 573-3, EN 485, EN 603

200 °C, 20 °C

2.43e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.43e-05 1/K

T62

EN 573-3, EN 485, EN 603

100 °C, 20 °C

2.3399999999999996e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3399999999999996e-05 1/K

T62

EN 573-3, EN 485, EN 603

20 °C, -50 °C

2.16e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.16e-05 1/K

T62

EN 573-3, EN 485, EN 603

Melting point

480.0 - 640.0 °C

Show Material materials with Melting point of 480.0 - 640.0 °C

T62

EN 573-3, EN 485, EN 603

Specific heat capacity

862.0 J/(kg·K)

Show Material materials with Specific heat capacity of 862.0 J/(kg·K)

T62

EN 573-3, EN 485, EN 603

Thermal conductivity

130.0 - 160.0 W/(m·K)

Show Material materials with Thermal conductivity of 130.0 - 160.0 W/(m·K)

T62

EN 573-3, EN 485, EN 603

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

19000000.0 - 23000000.0 S/m

Show Material materials with Electrical conductivity of 19000000.0 - 23000000.0 S/m

T62

EN 573-3, EN 485, EN 603

Electrical resistivity

4.35e-08 - 5.26e-08 Ω·m

Show Material materials with Electrical resistivity of 4.35e-08 - 5.26e-08 Ω·m

T62

EN 573-3, EN 485, EN 603

Chemical properties

PropertyValueConditionRelated Standards

Chromium

0.18 - 0.28 %

Show Material materials with Chromium of 0.18 - 0.28 %

T62

EN 573-3, EN 485, EN 603

Copper

1.2 - 2.0 %

Show Material materials with Copper of 1.2 - 2.0 %

T62

EN 573-3, EN 485, EN 603

Iron

0.50 %

Show Material materials with Iron of 0.50 %

T62

EN 573-3, EN 485, EN 603

Magnesium

2.1 - 2.9 %

Show Material materials with Magnesium of 2.1 - 2.9 %

T62

EN 573-3, EN 485, EN 603

Manganese

0.3 %

Show Material materials with Manganese of 0.3 %

T62

EN 573-3, EN 485, EN 603

Silicon

0.4 %

Show Material materials with Silicon of 0.4 %

T62

EN 573-3, EN 485, EN 603

Titanium

0.2 %

Show Material materials with Titanium of 0.2 %

T62

EN 573-3, EN 485, EN 603

Zinc

5.1 - 6.1 %

Show Material materials with Zinc of 5.1 - 6.1 %

T62

EN 573-3, EN 485, EN 603

Technological properties

Property
Anodizing

decorative: not suitable, Protective: acceptable

Brazing

hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: not suitable, soft brazing with flux: not suitable

Corrosion properties

Seawater: sufficient to poor, weathering: sufficient to poor

Workability

Bending / Spinning (cold): sufficient (O) / not suitable, Impact extrusion (cold): not suitable, Deep drawing / upsetting (Condition) not suitable / not suitable