General
Mechanical
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 25.0 MPa Show Material materials with Bending Fatigue Strength of 25.0 MPa | H14 | EN 573-3, EN 683 | |||
35.0 MPa Show Material materials with Bending Fatigue Strength of 35.0 MPa | H14 | EN 573-3, EN 1301, EN 485, EN 754 | ||||
Bending angle 180° | 1.0 °/t Show Material materials with Bending angle 180° of 1.0 °/t | H14 | EN 573-3, EN 485 | |||
Bending angle 90° | 0.5 °/t Show Material materials with Bending angle 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | |||
1.0 °/t Show Material materials with Bending angle 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | ||||
1.5 °/t Show Material materials with Bending angle 90° of 1.5 °/t | H14 | EN 573-3, EN 485 | ||||
2.5 °/t Show Material materials with Bending angle 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | ||||
Elastic modulus | -195.0 °C | 78.4 GPa Show Material materials with Elastic modulus of 78.4 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
-85.0 °C | 73.5 GPa Show Material materials with Elastic modulus of 73.5 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
-30.0 °C | 71.4 GPa Show Material materials with Elastic modulus of 71.4 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
69.0 GPa Show Material materials with Elastic modulus of 69.0 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Elastic modulus of 60.0 - 70.0 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Elastic modulus of 70.0 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
100.0 °C | 68.6 GPa Show Material materials with Elastic modulus of 68.6 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
150.0 °C | 66.5 GPa Show Material materials with Elastic modulus of 66.5 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Elastic modulus of 63.0 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
250.0 °C | 56.0 GPa Show Material materials with Elastic modulus of 56.0 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Elongation | 1.0 % Show Material materials with Elongation of 1.0 % | H14 | EN 573-3, EN 683 | A50 | ||
2.0 % Show Material materials with Elongation of 2.0 % | H14 | EN 573-3, EN 485, EN 683 | A50 | |||
4.0 % Show Material materials with Elongation of 4.0 % | H14 | EN 573-3, EN 485 | A50 | |||
5.0 % Show Material materials with Elongation of 5.0 % | H14 | EN 573-3, EN 1301 | ||||
5.0 % Show Material materials with Elongation of 5.0 % | H14 | EN 573-3, EN 485, EN 754 | A50 | |||
6.0 % Show Material materials with Elongation of 6.0 % | H14 | EN 573-3, EN 485, EN 754 | A100 | |||
6.0 % Show Material materials with Elongation of 6.0 % | H14 | EN 573-3, EN 485 | A50 | |||
20.0 °C | 1.0 % Show Material materials with Elongation of 1.0 % | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A100 | |
20.0 °C | 2.0 % Show Material materials with Elongation of 2.0 % | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Flat | A10 | |
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | A10 | |
20.0 °C | 4.0 % Show Material materials with Elongation of 4.0 % | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Wire | A100 | |
20.0 °C | 5.0 % Show Material materials with Elongation of 5.0 % | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Tube | A10 | |
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Wire | A10 | |
20.0 °C | 6.0 % Show Material materials with Elongation of 6.0 % | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip, Tube | ||
20.0 °C | 7.0 % Show Material materials with Elongation of 7.0 % | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod | ||
Hardness, Brinell | 34.0 [-] Show Material materials with Hardness, Brinell of 34.0 [-] | H14 | EN 573-3, EN 485 | |||
20.0 °C | 28.0 [-] Show Material materials with Hardness, Brinell of 28.0 [-] | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Tube | ||
20.0 °C | 30.0 [-] Show Material materials with Hardness, Brinell of 30.0 [-] | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Wire | ||
20.0 °C | 35.0 [-] Show Material materials with Hardness, Brinell of 35.0 [-] | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Shear modulus | 25.9 GPa Show Material materials with Shear modulus of 25.9 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | |||
20.0 °C | 25.0 - 26.5 GPa Show Material materials with Shear modulus of 25.0 - 26.5 GPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | ||
Shear strength | 20.0 °C | 55.0 MPa Show Material materials with Shear strength of 55.0 MPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Wire | |
Tensile strength | 100.0 MPa Show Material materials with Tensile strength of 100.0 MPa | H14 | EN 573-3, EN 1301 | |||
100.0 - 135.0 MPa Show Material materials with Tensile strength of 100.0 - 135.0 MPa | H14 | EN 573-3, EN 754 | ||||
105.0 - 145.0 MPa Show Material materials with Tensile strength of 105.0 - 145.0 MPa | H14 | EN 573-3, EN 485, EN 683 | ||||
20.0 °C | 100.0 MPa Show Material materials with Tensile strength of 100.0 MPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Tube, Wire | ||
20.0 °C | 110.0 - 150.0 MPa Show Material materials with Tensile strength of 110.0 - 150.0 MPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Sheet, Flat, Strip | ||
20.0 °C | 170.0 - 210.0 MPa Show Material materials with Tensile strength of 170.0 - 210.0 MPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Flat | ||
20.0 °C | 180.0 MPa Show Material materials with Tensile strength of 180.0 MPa | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Flat |
Thermal
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Coefficient of thermal expansion | -50 °C | 2.17e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
-50.0 °C | 2.17e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
20 °C | 2.17e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.17e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
20 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
100 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
100.0 °C | 2.35e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754, DIN 1712-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
200.0 °C | 2.44e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.44e-05 1/K | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
300.0 °C | 2.54e-05 1/K Show Material materials with Coefficient of thermal expansion of 2.54e-05 1/K | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Melting point | 646.0 - 657.0 °C Show Material materials with Melting point of 646.0 - 657.0 °C | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
Specific heat capacity | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Specific heat capacity of 900.0 J/(kg·K) | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Thermal conductivity | 20.0 °C | 210.0 - 220.0 W/(m·K) Show Material materials with Thermal conductivity of 210.0 - 220.0 W/(m·K) | H14 | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Electrical
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Electrical conductivity | 34000000.0 - 36000000.0 S/m Show Material materials with Electrical conductivity of 34000000.0 - 36000000.0 S/m | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
20.0 °C | 34800000.0 - 36000000.0 S/m Show Material materials with Electrical conductivity of 34800000.0 - 36000000.0 S/m | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire | |
Electrical resistivity | 2.78e-08 - 2.94e-08 Ω·m Show Material materials with Electrical resistivity of 2.78e-08 - 2.94e-08 Ω·m | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | |
Copper | 0.05 % Show Material materials with Copper of 0.05 % | H14 | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Iron | 0.4 % Show Material materials with Iron of 0.4 % | H14 | DIN 1712-3, EN 573-3, EN 573-4 | Rod, Sheet, Flat, Strip, Tube, Wire |
0.40 % Show Material materials with Iron of 0.40 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | ||
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | H14 | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Manganese | 0.05 % Show Material materials with Manganese of 0.05 % | H14 | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Silicon | 0.25 % Show Material materials with Silicon of 0.25 % | H14 | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Titanium | 0.05 % Show Material materials with Titanium of 0.05 % | H14 | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Zinc | 0.07 % Show Material materials with Zinc of 0.07 % | H14 | DIN 1712-3, EN 573-3, EN 573-4, EN 1301, EN 485, EN 683, EN 754 | Rod, Sheet, Flat, Strip, Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: acceptable, weathering: good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |