DIN 1712-3 Grade 3.0257 O

Want to keep this datasheet? Save it now in your required format

Description

Pure aluminium Electrical conductivity alloy according to DIN, ensured by the German electrotechnical commission for electro-technology with, also in accordance to DIN 40 501 part of 1 to part of 4. This material has a very good electrical and good thermal conductivity, however only relatively low mechanical strength. Forming capacity and chemical as well as weather proofness are very good. Application: Roll bond, z-bond, wiring loom-change with particularly high requirements.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyTemperatureValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

O

EN 573-3, EN 485, EN 755

20.0 °C

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

O

DIN 1712-3, EN 573-3, EN 573-4

Wire, Sheet, Strip

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

O

EN 573-3, EN 485, EN 755

Elongation

20.0 %

Show Material materials with Elongation of 20.0 %

O

EN 573-3, EN 485

A50

22.0 %

Show Material materials with Elongation of 22.0 %

O

EN 573-3, EN 485, EN 755

A50

25.0 %

Show Material materials with Elongation of 25.0 %

O

EN 573-3, EN 755

A100

26.0 %

Show Material materials with Elongation of 26.0 %

O

EN 573-3, EN 485

A50

29.0 %

Show Material materials with Elongation of 29.0 %

O

EN 573-3, EN 485

A50

32.0 %

Show Material materials with Elongation of 32.0 %

O

EN 573-3, EN 485

A100

35.0 %

Show Material materials with Elongation of 35.0 %

O

EN 573-3, EN 485

A50

20.0 °C

16.0 %

Show Material materials with Elongation of 16.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

A200

20.0 °C

18.0 %

Show Material materials with Elongation of 18.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

A100

20.0 °C

20.0 %

Show Material materials with Elongation of 20.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

A200

20.0 °C

22.0 %

Show Material materials with Elongation of 22.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

A100

20.0 °C

23.0 %

Show Material materials with Elongation of 23.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

A200

20.0 °C

25.0 %

Show Material materials with Elongation of 25.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

A100

20.0 °C

30.0 %

Show Material materials with Elongation of 30.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

A100

20.0 °C

35.0 %

Show Material materials with Elongation of 35.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Sheet, Strip

A10

20.0 °C

40.0 %

Show Material materials with Elongation of 40.0 %

O

DIN 1712-3, EN 573-3, EN 573-4

Sheet, Strip

Hardness, Brinell

20.0 [-]

Show Material materials with Hardness, Brinell of 20.0 [-]

O

EN 573-3, EN 485, EN 755

20.0 °C

18.0 - 26.0 [-]

Show Material materials with Hardness, Brinell of 18.0 - 26.0 [-]

O

DIN 1712-3, EN 573-3, EN 573-4

Sheet, Strip

Hardness, Vickers

20.0 °C

20.0 - 30.0 [-]

Show Material materials with Hardness, Vickers of 20.0 - 30.0 [-]

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 1000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 1000 Series Aluminium

Shear modulus

20.0 °C

25.0 - 26.5 GPa

Show Material materials with Shear modulus of 25.0 - 26.5 GPa

O

DIN 1712-3, EN 573-3, EN 573-4

Wire, Sheet, Strip

Tensile strength

60.0 MPa

Show Material materials with Tensile strength of 60.0 MPa

O

EN 573-3, EN 755

65.0 - 105.0 MPa

Show Material materials with Tensile strength of 65.0 - 105.0 MPa

O

EN 573-3, EN 485

20.0 °C

60.0 - 90.0 MPa

Show Material materials with Tensile strength of 60.0 - 90.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

20.0 °C

60.0 - 80.0 MPa

Show Material materials with Tensile strength of 60.0 - 80.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

20.0 °C

60.0 - 120.0 MPa

Show Material materials with Tensile strength of 60.0 - 120.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

20.0 °C

60.0 - 100.0 MPa

Show Material materials with Tensile strength of 60.0 - 100.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

20.0 °C

65.0 - 95.0 MPa

Show Material materials with Tensile strength of 65.0 - 95.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Sheet, Strip

20.0 °C

70.0 - 120.0 MPa

Show Material materials with Tensile strength of 70.0 - 120.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

20.0 °C

70.0 - 100.0 MPa

Show Material materials with Tensile strength of 70.0 - 100.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

20.0 °C

70.0 - 90.0 MPa

Show Material materials with Tensile strength of 70.0 - 90.0 MPa

O

DIN 1712-3, EN 573-3, EN 573-4

Wire

Thermal

PropertyTemperatureValueConditionRelated StandardsShape

Coefficient of thermal expansion

20 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 485, EN 755

100 °C

2.35e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.35e-05 1/K

O

EN 573-3, EN 485, EN 755

Melting point

658.0 °C

Show Material materials with Melting point of 658.0 °C

O

EN 573-3, EN 485, EN 755

Specific heat capacity

20.0 °C

921.0 J/(kg·K)

Show Material materials with Specific heat capacity of 921.0 J/(kg·K)

O

DIN 1712-3, EN 573-3, EN 573-4

Wire, Sheet, Strip

Thermal conductivity

230 W/(m·K)

Show Material materials with Thermal conductivity of 230 W/(m·K)

O

EN 573-3, EN 485, EN 755

20.0 °C

230.0 W/(m·K)

Show Material materials with Thermal conductivity of 230.0 W/(m·K)

O

DIN 1712-3, EN 573-3, EN 573-4

Wire, Sheet, Strip

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

34500000.0 - 35500000.0 S/m

Show Material materials with Electrical conductivity of 34500000.0 - 35500000.0 S/m

O

EN 573-3, EN 485, EN 755

Electrical resistivity

2.82e-08 - 2.9e-08 Ω·m

Show Material materials with Electrical resistivity of 2.82e-08 - 2.9e-08 Ω·m

O

EN 573-3, EN 485, EN 755

Chemical properties

PropertyValueConditionRelated StandardsShape

Aluminium

99.5 %

Show Material materials with Aluminium of 99.5 %

O

EN 573-3, EN 485, EN 755

Copper

0.02 %

Show Material materials with Copper of 0.02 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 755

Wire, Sheet, Strip

Iron

0.4 %

Show Material materials with Iron of 0.4 %

O

DIN 1712-3, EN 573-3, EN 573-4

Wire, Sheet, Strip

0.40 %

Show Material materials with Iron of 0.40 %

O

EN 573-3, EN 485, EN 755

Magnesium

0.05 %

Show Material materials with Magnesium of 0.05 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 755

Wire, Sheet, Strip

Silicon

0.25 %

Show Material materials with Silicon of 0.25 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 755

Wire, Sheet, Strip

Zinc

0.05 %

Show Material materials with Zinc of 0.05 %

O

DIN 1712-3, EN 573-3, EN 573-4, EN 485, EN 755

Wire, Sheet, Strip

Technological properties

Property
Brazing

Excellent

Workability

Excellent workability.