AA Standards Grade 2014 T6

Want to keep this datasheet? Save it now in your required format

Description

AA 2014 is an alloy with strength, machinability and welding capabilities, Aluminum Alloy AA 2014 is an excellent option. It is a precipitation hardening alloy that maintains strength after heat treatment.

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.8 g/cm³

Show Material materials with Density of 2.8 g/cm³

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Mechanical

PropertyTemperatureValueConditionRelated StandardsComment

Bending Fatigue Strength

125.0 MPa

Show Material materials with Bending Fatigue Strength of 125.0 MPa

T6

AA Standards

Unlock all property charts

Elastic modulus

73.0 GPa

Show Material materials with Elastic modulus of 73.0 GPa

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Unlock all property charts

Elongation A100

23.0 °C

1 - 11 %

Show Material materials with Elongation A100 of 1 - 11 %

Elongation A50

23.0 °C

2 - 8 %

Show Material materials with Elongation A50 of 2 - 8 %

Hardness, Brinell

135.0 [-]

Show Material materials with Hardness, Brinell of 135.0 [-]

T6

AA Standards

Unlock all property charts

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 2000 Series Aluminium

Unlock all property charts

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 2000 Series Aluminium

Unlock all property charts

Shear modulus

26.0 - 27.5 GPa

Show Material materials with Shear modulus of 26.0 - 27.5 GPa

Typical for Wrought 2000 Series Aluminium

Unlock all property charts

Tensile strength

485.0 MPa

Show Material materials with Tensile strength of 485.0 MPa

T6

AA Standards

435.0 MPa

Show Material materials with Tensile strength of 435.0 MPa

T6

AA Standards, ASTM B209, ASTM B247

460.0 MPa

Show Material materials with Tensile strength of 460.0 MPa

T6

AA Standards, ASTM B209

450.0 MPa

Show Material materials with Tensile strength of 450.0 MPa

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B247

440.0 MPa

Show Material materials with Tensile strength of 440.0 MPa

T6

AA Standards, ASTM B209, ASTM B241, ASTM B247

455.0 MPa

Show Material materials with Tensile strength of 455.0 MPa

T6

AA Standards, ASTM B209

405.0 MPa

Show Material materials with Tensile strength of 405.0 MPa

T6

AA Standards, ASTM B209, ASTM B247

470.0 MPa

Show Material materials with Tensile strength of 470.0 MPa

T6

AA Standards, ASTM B241

415.0 MPa

Show Material materials with Tensile strength of 415.0 MPa

T6

AA Standards, ASTM B241, ASTM B247

420.0 MPa

Show Material materials with Tensile strength of 420.0 MPa

T6

AA Standards, ASTM B247

425.0 MPa

Show Material materials with Tensile strength of 425.0 MPa

T6

AA Standards, ASTM B247

400.0 MPa

Show Material materials with Tensile strength of 400.0 MPa

T6

AA Standards, ASTM B247

395.0 MPa

Show Material materials with Tensile strength of 395.0 MPa

T6

AA Standards, ASTM B247

Unlock all property charts

Yield strength Rp0.2

23.0 °C

350 - 415 MPa

Show Material materials with Yield strength Rp0.2 of 350 - 415 MPa

Thermal

PropertyTemperatureValueConditionRelated StandardsComment

Coefficient of thermal expansion

100 °C, 20 °C

2.3e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3e-05 1/K

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Unlock all property charts

Melting point

505.0 - 635.0 °C

Show Material materials with Melting point of 505.0 - 635.0 °C

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Specific heat capacity

816.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 816.0 - 963.0 J/(kg·K)

Typical for Wrought 2000 Series Aluminium

Unlock all property charts

Thermal conductivity

134.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 134.0 - 193.0 W/(m·K)

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Unlock all property charts

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

20000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 20000000.0 - 29000000.0 S/m

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Unlock all property charts

Electrical resistivity

3.45e-08 - 5e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 5e-08 Ω·m

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Unlock all property charts

Chemical properties

PropertyValueConditionRelated Standards

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Copper

3.9 - 5.0 %

Show Material materials with Copper of 3.9 - 5.0 %

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Iron

0.70 %

Show Material materials with Iron of 0.70 %

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Magnesium

0.2 - 0.8 %

Show Material materials with Magnesium of 0.2 - 0.8 %

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Manganese

0.4 - 1.2 %

Show Material materials with Manganese of 0.4 - 1.2 %

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Other

each 0.05, total 0.15, Rest Al

Silicon

0.5 - 1.2 %

Show Material materials with Silicon of 0.5 - 1.2 %

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Titanium

0.15 %

Show Material materials with Titanium of 0.15 %

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

T6

AA Standards, ASTM B209, ASTM B210, ASTM B211, ASTM B241, ASTM B247

Technological properties

Property
Brazing

general: no brazing is known or developed

Corrosion properties

Stress corrosion cracking: Operational damage in areas with tensile stresses transverse to the grain structure, limited damage to laboratory samples, general: sufficient, in principle it should be protected

General machinability

General: poor (O), good to acceptable

Workability

general (condition): poor(T3, T4, T451), not suitable (T6, T651, T6510, T6511)