General
Property | Value | Temperature |
---|---|---|
Density | 2.79 g/cm³ Show Material materials with Density of 2.79 g/cm³ at 23.0 °C | 23.0 °C |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Elastic modulus | 73 GPa Show Material materials with Elastic modulus of 73 GPa at 23.0 °C | 23.0 °C | |
Elongation A100 | 10 % Show Material materials with Elongation A100 of 10 % at 23.0 °C | 23.0 °C | |
Elongation A50 | 12 % Show Material materials with Elongation A50 of 12 % at 23.0 °C | 23.0 °C | |
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 2000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C | 23.0 °C | Typical for Wrought 2000 Series Aluminium |
Shear modulus | 26 - 27.5 GPa Show Material materials with Shear modulus of 26 - 27.5 GPa at 23.0 °C | 23.0 °C | Typical for Wrought 2000 Series Aluminium |
Tensile strength | 380 MPa Show Material materials with Tensile strength of 380 MPa at 23.0 °C | 23.0 °C | |
Yield strength Rp0.2 | 220 MPa Show Material materials with Yield strength Rp0.2 of 220 MPa at 23.0 °C | 23.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.36E-5 1/K at 20.0 °C | 20.0 °C | |
2.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.36E-5 1/K at 100.0 °C | 100.0 °C | ||
Melting point | 510 - 640 °C Show Material materials with Melting point of 510 - 640 °C | ||
Specific heat capacity | 816 - 963 J/(kg·K) Show Material materials with Specific heat capacity of 816 - 963 J/(kg·K) at 23.0 °C | 23.0 °C | Typical for Wrought 2000 Series Aluminium |
Thermal conductivity | 134 - 193 W/(m·K) Show Material materials with Thermal conductivity of 134 - 193 W/(m·K) at 23.0 °C | 23.0 °C |
Electrical
Property | Value | Temperature |
---|---|---|
Electrical conductivity | 2.00E+7 - 2.90E+7 S/m Show Material materials with Electrical conductivity of 2.00E+7 - 2.90E+7 S/m at 23.0 °C | 23.0 °C |
Electrical resistivity | 3.45E-8 - 5E-8 Ω·m Show Material materials with Electrical resistivity of 3.45E-8 - 5E-8 Ω·m at 23.0 °C | 23.0 °C |
Chemical properties
Property | ||
---|---|---|
Chromium | 0.1 % | |
Copper | 3.5 - 4.5 % | |
Iron | 0.7 % | |
Magnesium | 0.4 - 0.8 % | |
Manganese | 0.4 - 1 % | |
Other | each 0.05, total 0.15, Rest Al | |
Silicon | 0.2 - 0.8 % | |
Titanium | 0.15 % | |
Zinc | 0.25 % |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Operational damage in areas with tensile stresses transverse to the grain structure, limited damage to laboratory samples, general: sufficient, in principle it should be protected | |
General machinability | General: good to acceptable | |
Workability | general (condition): poor(T4, T451) |