General
Property | Value | Temperature |
---|---|---|
Density | 2.71 g/cm³ Show Material materials with Density of 2.71 g/cm³ at 23.0 °C | 23.0 °C |
Mechanical
Property | Value | Temperature | Comment |
---|---|---|---|
Bending Fatigue Strength | 30 MPa Show Material materials with Bending Fatigue Strength of 30 MPa at 23.0 °C | 23.0 °C | |
Elastic modulus | 69 GPa Show Material materials with Elastic modulus of 69 GPa at 23.0 °C | 23.0 °C | |
Elongation A100 | 10 % Show Material materials with Elongation A100 of 10 % at 23.0 °C | 23.0 °C | |
Elongation A50 | 6 - 16 % Show Material materials with Elongation A50 of 6 - 16 % at 23.0 °C | 23.0 °C | |
Hardness, Brinell | 23 [-] Show Material materials with Hardness, Brinell of 23 [-] at 23.0 °C | 23.0 °C | |
Plane-Strain Fracture Toughnes | 22 - 35 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22 - 35 MPa·√m at 23.0 °C | 23.0 °C | Typical for Wrought 1000 Series Aluminium |
Poisson's ratio | 0.33 [-] Show Material materials with Poisson's ratio of 0.33 [-] at 23.0 °C | 23.0 °C | Typical for Wrought 1000 Series Aluminium |
Shear modulus | 25.9 GPa Show Material materials with Shear modulus of 25.9 GPa at 23.0 °C | 23.0 °C | Typical for Wrought 1000 Series Aluminium |
Tensile strength | 70 - 110 MPa Show Material materials with Tensile strength of 70 - 110 MPa at 23.0 °C | 23.0 °C | |
Yield strength Rp0.2 | 30 - 75 MPa Show Material materials with Yield strength Rp0.2 of 30 - 75 MPa at 23.0 °C | 23.0 °C |
Thermal
Property | Value | Temperature | Comment |
---|---|---|---|
Coefficient of thermal expansion | 2.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.36E-5 1/K at 20.0 °C | 20.0 °C | |
2.36E-5 1/K Show Material materials with Coefficient of thermal expansion of 2.36E-5 1/K at 100.0 °C | 100.0 °C | ||
Melting point | 645 - 655 °C Show Material materials with Melting point of 645 - 655 °C | ||
Specific heat capacity | 900 - 963 J/(kg·K) Show Material materials with Specific heat capacity of 900 - 963 J/(kg·K) at 23.0 °C | 23.0 °C | Typical for Wrought 1000 Series Aluminium |
Thermal conductivity | 230 - 234 W/(m·K) Show Material materials with Thermal conductivity of 230 - 234 W/(m·K) at 23.0 °C | 23.0 °C |
Electrical
Property | Value | Temperature |
---|---|---|
Electrical conductivity | 3.50E+7 - 3.60E+7 S/m Show Material materials with Electrical conductivity of 3.50E+7 - 3.60E+7 S/m at 23.0 °C | 23.0 °C |
Electrical resistivity | 2.78E-8 - 2.86E-8 Ω·m Show Material materials with Electrical resistivity of 2.78E-8 - 2.86E-8 Ω·m at 23.0 °C | 23.0 °C |
Chemical properties
Property | ||
---|---|---|
Aluminium | 99.6 % | |
Copper | 0.05 % | |
Iron | 0.35 % | |
Magnesium | 0.03 % | |
Manganese | 0.03 % | |
Other | each 0.03 | |
Silicon | 0.25 % | |
Titanium | 0.03 % | |
Vanadium | 0.05 % | |
Zinc | 0.05 % |
Technological properties
Property | ||
---|---|---|
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: not suitable (O, H12), poor (H14, H16, H18) | |
Workability | general (condition): good (O, H12, H14), acceptable (H16, H18) |