AA Standards Grade 3003 H112

View suppliers (176)
Want to keep this datasheet? Save it now in your required format

Description

Aluminum AA 3003 is a popular alloy that offers customers very good atmospheric corrosion resistance and moderate strength. Aluminum 3003 offers good machinability for aluminum alloys, though it is not heat treatable. Unlike other aluminum alloys, AA 3003 is weldable by conventional welding methods. It also takes cold and hot working well and has generally better mechanical properties when compared to 1000 series aluminum alloys.

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.73 g/cm³

Show Material materials with Density of 2.73 g/cm³

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 3000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 3000 Series Aluminium

Shear modulus

25.0 - 26.0 GPa

Show Material materials with Shear modulus of 25.0 - 26.0 GPa

Typical for Wrought 3000 Series Aluminium

Tensile strength

90.0 MPa

Show Material materials with Tensile strength of 90.0 MPa

H112

AA Standards, ASTM B221

95.0 MPa

Show Material materials with Tensile strength of 95.0 MPa

H112

AA Standards, ASTM B211, ASTM B241, ASTM B247, ASTM B345, ASTM B483

100.0 MPa

Show Material materials with Tensile strength of 100.0 MPa

H112

AA Standards, ASTM B209

105.0 MPa

Show Material materials with Tensile strength of 105.0 MPa

H112

AA Standards, ASTM B209

115.0 MPa

Show Material materials with Tensile strength of 115.0 MPa

H112

AA Standards, ASTM B209, ASTM B547

Thermal

PropertyTemperatureValueConditionRelated StandardsComment

Coefficient of thermal expansion

20 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

100 °C

2.3199999999999998e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.3199999999999998e-05 1/K

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Melting point

640.0 - 655.0 °C

Show Material materials with Melting point of 640.0 - 655.0 °C

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Specific heat capacity

893.0 - 920.0 J/(kg·K)

Show Material materials with Specific heat capacity of 893.0 - 920.0 J/(kg·K)

Typical for Wrought 3000 Series Aluminium

Thermal conductivity

159.0 - 193.0 W/(m·K)

Show Material materials with Thermal conductivity of 159.0 - 193.0 W/(m·K)

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

24000000.0 - 29000000.0 S/m

Show Material materials with Electrical conductivity of 24000000.0 - 29000000.0 S/m

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Electrical resistivity

3.45e-08 - 4.17e-08 Ω·m

Show Material materials with Electrical resistivity of 3.45e-08 - 4.17e-08 Ω·m

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Chemical properties

PropertyValueConditionRelated Standards

Copper

0.05 - 0.2 %

Show Material materials with Copper of 0.05 - 0.2 %

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Iron

0.70 %

Show Material materials with Iron of 0.70 %

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Manganese

1.0 - 1.5 %

Show Material materials with Manganese of 1.0 - 1.5 %

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Silicon

0.6 %

Show Material materials with Silicon of 0.6 %

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

H112

AA Standards, ASTM B209, ASTM B211, ASTM B221, ASTM B241, ASTM B247, ASTM B345, ASTM B483, ASTM B547

Technological properties

Property
Brazing

general: possible with commercial processes and methods

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere

General machinability

General: not suitable (O, H12), poor (H14, H16, H25)

Workability

general (condition): good (O, H12), acceptable (H14, H25), poor(H16, H18)