AA Standards Grade 5005 H38

Want to keep this datasheet? Save it now in your required format

Description

Aluminum AA 5005 is a lean aluminum magnesium alloy with low density and excellent thermal conductivity. This medium strength non-heat-treatable alloy is known for its corrosion resistance in alkaline marine situations. Aluminum AA 5005 is readily machinable, and can be welded using TIG and MIG methods. It is important to note that anodizing is a critical part to how Aluminum AA 5005 is used.

Related Standards

Equivalent Materials

This material data has been provided by AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated Standards

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

H38

AA Standards, ASTM B209

Mechanical

PropertyValueConditionRelated StandardsComment

Elastic modulus

69.0 GPa

Show Material materials with Elastic modulus of 69.0 GPa

H38

AA Standards, ASTM B209

Hardness, Brinell

51.0 [-]

Show Material materials with Hardness, Brinell of 51.0 [-]

H38

AA Standards

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 5000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 5000 Series Aluminium

Shear modulus

26.0 - 26.5 GPa

Show Material materials with Shear modulus of 26.0 - 26.5 GPa

Typical for Wrought 5000 Series Aluminium

Tensile strength

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

H38

AA Standards, ASTM B209

200.0 MPa

Show Material materials with Tensile strength of 200.0 MPa

H38

AA Standards

Thermal

PropertyTemperatureValueConditionRelated StandardsComment

Coefficient of thermal expansion

20 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H38

AA Standards, ASTM B209

100 °C

2.38e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.38e-05 1/K

H38

AA Standards, ASTM B209

Max service temperature

150.0 °C

Show Material materials with Max service temperature of 150.0 °C

Typical for Wrought 5000 Series Aluminium

Melting point

630.0 - 655.0 °C

Show Material materials with Melting point of 630.0 - 655.0 °C

H38

AA Standards, ASTM B209

Specific heat capacity

879.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 879.0 - 963.0 J/(kg·K)

Typical for Wrought 5000 Series Aluminium

Thermal conductivity

201 W/(m·K)

Show Material materials with Thermal conductivity of 201 W/(m·K)

H38

AA Standards, ASTM B209

Electrical

PropertyValueConditionRelated Standards

Electrical conductivity

30000000.0 S/m

Show Material materials with Electrical conductivity of 30000000.0 S/m

H38

AA Standards, ASTM B209

Electrical resistivity

3.33e-08 Ω·m

Show Material materials with Electrical resistivity of 3.33e-08 Ω·m

H38

AA Standards, ASTM B209

Chemical properties

PropertyValueConditionRelated Standards

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

H38

AA Standards, ASTM B209

Copper

0.2 %

Show Material materials with Copper of 0.2 %

H38

AA Standards, ASTM B209

Iron

0.70 %

Show Material materials with Iron of 0.70 %

H38

AA Standards, ASTM B209

Magnesium

0.5 - 1.1 %

Show Material materials with Magnesium of 0.5 - 1.1 %

H38

AA Standards, ASTM B209

Manganese

0.2 %

Show Material materials with Manganese of 0.2 %

H38

AA Standards, ASTM B209

Silicon

0.3 %

Show Material materials with Silicon of 0.3 %

H38

AA Standards, ASTM B209

Zinc

0.25 %

Show Material materials with Zinc of 0.25 %

H38

AA Standards, ASTM B209

Technological properties

Property
Brazing

general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen

Corrosion properties

Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere

General machinability

General: not suitable (O, H12, H32), poor (H14, H34, H16, H18, H36, H38)

Workability

general (condition): good (O, H12, H32), acceptable (H14, H34), poor(H16, H18, H36, H38)