General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.23 g/cm³ Show Supplier Material materials with Density of 1.23 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 0.16 % Show Supplier Material materials with Moisture absorption of 0.16 % | dry | Sim. to ISO 62 | |
Water absorption | 0.48 % Show Supplier Material materials with Water absorption of 0.48 % | dry | ISO 62 | at 23°C after 24h |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elastic modulus | 0.26 GPa Show Supplier Material materials with Elastic modulus of 0.26 GPa | dry | ISO 527-1/-2 | ||
Elongation | 50 % Show Supplier Material materials with Elongation of 50 % | dry | ISO 527-1/-2 | ||
Hardness, Shore A | 98 [-] Show Supplier Material materials with Hardness, Shore A of 98 [-] | dry | ISO 868 | 3s | |
98 [-] Show Supplier Material materials with Hardness, Shore A of 98 [-] | dry | ISO 868 | 15s | ||
Hardness, Shore D | 57.0 [-] Show Supplier Material materials with Hardness, Shore D of 57.0 [-] | dry | ISO 868 | 3s | |
57.0 [-] Show Supplier Material materials with Hardness, Shore D of 57.0 [-] | dry | ISO 868 | 15s | ||
Impact strength, Charpy notched | -30 °C | 11 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 11 kJ/m² | dry | ISO 179/1eA | |
23 °C | 21 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 21 kJ/m² | dry | ISO 179/1eA | ||
Tear strength | 148 kN/m Show Supplier Material materials with Tear strength of 148 kN/m | dry | ISO 34-1; Method B | ||
Tensile strength | 31 MPa Show Supplier Material materials with Tensile strength of 31 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Glass transition temperature | -30 °C Show Supplier Material materials with Glass transition temperature of -30 °C | dry | ASTM D5026/D7028 | DMTA (E) |
Melting point | 212 °C Show Supplier Material materials with Melting point of 212 °C | dry | ISO 11357-1/-3 | 10°C/min |
Vicat softening temperature | 110 °C Show Supplier Material materials with Vicat softening temperature of 110 °C | dry | ISO 306 | 50°C/h 50N |
200 °C Show Supplier Material materials with Vicat softening temperature of 200 °C | dry | ISO 306 | 50°C/h 10N |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Melt volume-flow rate | 230 °C | 3 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 3 cm³/10min | dry | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Application areas | Brake Tubing with Arnitel® CM622 |