General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.65 g/cm³ Show Supplier Material materials with Density of 1.65 g/cm³ | dry | ISO 1183 |
Moisture absorption | 0.15 % Show Supplier Material materials with Moisture absorption of 0.15 % | dry | Sim. to ISO 62 |
Water absorption | 0.3 % Show Supplier Material materials with Water absorption of 0.3 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | -40 °C | 1.2 GPa Show Supplier Material materials with Elastic modulus of 1.2 GPa | dry | ISO 527-1/-2 |
11 GPa Show Supplier Material materials with Elastic modulus of 11 GPa | dry | ISO 527-1/-2 | ||
100 °C | 5.3 GPa Show Supplier Material materials with Elastic modulus of 5.3 GPa | dry | ISO 527-1/-2 | |
120 °C | 4.6 GPa Show Supplier Material materials with Elastic modulus of 4.6 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.1 GPa Show Supplier Material materials with Elastic modulus of 3.1 GPa | dry | ISO 527-1/-2 | |
180 °C | 2.3 GPa Show Supplier Material materials with Elastic modulus of 2.3 GPa | dry | ISO 527-1/-2 | |
Elongation | -40 °C | 2.5 % Show Supplier Material materials with Elongation of 2.5 % | dry | ISO 527-1/-2 |
2.5 % Show Supplier Material materials with Elongation of 2.5 % | dry | ISO 527-1/-2 | ||
120 °C | 5 % Show Supplier Material materials with Elongation of 5 % | dry | ISO 527-1/-2 | |
160 °C | 6 % Show Supplier Material materials with Elongation of 6 % | dry | ISO 527-1/-2 | |
180 °C | 7 % Show Supplier Material materials with Elongation of 7 % | dry | ISO 527-1/-2 | |
Flexural modulus | 10.5 GPa Show Supplier Material materials with Flexural modulus of 10.5 GPa | dry | ISO 178 | |
120 °C | 4.8 GPa Show Supplier Material materials with Flexural modulus of 4.8 GPa | dry | ISO 178 | |
160 °C | 3.2 GPa Show Supplier Material materials with Flexural modulus of 3.2 GPa | dry | ISO 178 | |
Flexural yield strength | 200 MPa Show Supplier Material materials with Flexural yield strength of 200 MPa | dry | ISO 178 | |
120 °C | 100 MPa Show Supplier Material materials with Flexural yield strength of 100 MPa | dry | ISO 178 | |
160 °C | 70 MPa Show Supplier Material materials with Flexural yield strength of 70 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | -30 °C | 8 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 8 kJ/m² | dry | ISO 179/1eA |
23 °C | 8 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 8 kJ/m² | dry | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 40 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 40 kJ/m² | dry | ISO 179/1eU |
23 °C | 50 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 50 kJ/m² | dry | ISO 179/1eU | |
Tensile strength | -40 °C | 195 MPa Show Supplier Material materials with Tensile strength of 195 MPa | dry | ISO 527-1/-2 |
130 MPa Show Supplier Material materials with Tensile strength of 130 MPa | dry | ISO 527-1/-2 | ||
100 °C | 70 MPa Show Supplier Material materials with Tensile strength of 70 MPa | dry | ISO 527-1/-2 | |
120 °C | 60 MPa Show Supplier Material materials with Tensile strength of 60 MPa | dry | ISO 527-1/-2 | |
160 °C | 45 MPa Show Supplier Material materials with Tensile strength of 45 MPa | dry | ISO 527-1/-2 | |
180 °C | 35 MPa Show Supplier Material materials with Tensile strength of 35 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 3.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 3.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
7e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 7e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Flammability | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 2 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 0.75 mm | |||
Glow Wire Ignition Temperature | 700 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 700 °C | dry | IEC 60695-2-13 | 2 mm | ||
725 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 725 °C | dry | IEC 60695-2-13 | 0.75 mm | |||
Heat deflection temperature | 210 °C Show Supplier Material materials with Heat deflection temperature of 210 °C | dry | ISO 75-1/-2 | 2 MPa | ||
220 °C Show Supplier Material materials with Heat deflection temperature of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 225 °C Show Supplier Material materials with Melting point of 225 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 150 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 150 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 140 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 140 °C | dry | UL746B | 0.75 mm |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 300 V Show Supplier Material materials with Comparative tracking index of 300 V | dry | IEC 60112 | |
Dielectric constant | 3.8 [-] Show Supplier Material materials with Dielectric constant of 3.8 [-] | dry | IEC 62631-2-1 | 1MHz |
4 [-] Show Supplier Material materials with Dielectric constant of 4 [-] | dry | IEC 62631-2-1 | 100Hz | |
Dielectric strength | 28.0 kV/mm Show Supplier Material materials with Dielectric strength of 28.0 kV/mm | dry | IEC 60243-1 | |
Dissipation factor | 25 [-] Show Supplier Material materials with Dissipation factor of 25 [-] | dry | IEC 62631-2-1 | 100Hz |
140 [-] Show Supplier Material materials with Dissipation factor of 140 [-] | dry | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Bobbins | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber |