General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.45 g/cm³ Show Supplier Material materials with Density of 1.45 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.1 % Show Supplier Material materials with Moisture absorption of 2.1 % | dry | Sim. to ISO 62 | |
Water absorption | 0.4 % Show Supplier Material materials with Water absorption of 0.4 % | dry | ISO 62 | at 23°C after 24h |
5.4 % Show Supplier Material materials with Water absorption of 5.4 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | -40 °C | 11.6 GPa Show Supplier Material materials with Elastic modulus of 11.6 GPa | dry | ISO 527-1/-2 |
-40 °C | 11.9 GPa Show Supplier Material materials with Elastic modulus of 11.9 GPa | conditioned | ISO 527-1/-2 | |
11.3 GPa Show Supplier Material materials with Elastic modulus of 11.3 GPa | dry | ISO 527-1/-2 | ||
11.6 GPa Show Supplier Material materials with Elastic modulus of 11.6 GPa | conditioned | ISO 527-1/-2 | ||
40 °C | 10.9 GPa Show Supplier Material materials with Elastic modulus of 10.9 GPa | conditioned | ISO 527-1/-2 | |
40 °C | 11 GPa Show Supplier Material materials with Elastic modulus of 11 GPa | dry | ISO 527-1/-2 | |
80 °C | 6.5 GPa Show Supplier Material materials with Elastic modulus of 6.5 GPa | conditioned | ISO 527-1/-2 | |
80 °C | 10.5 GPa Show Supplier Material materials with Elastic modulus of 10.5 GPa | dry | ISO 527-1/-2 | |
100 °C | 5.3 GPa Show Supplier Material materials with Elastic modulus of 5.3 GPa | conditioned | ISO 527-1/-2 | |
100 °C | 10 GPa Show Supplier Material materials with Elastic modulus of 10 GPa | dry | ISO 527-1/-2 | |
120 °C | 4.8 GPa Show Supplier Material materials with Elastic modulus of 4.8 GPa | conditioned | ISO 527-1/-2 | |
120 °C | 7.8 GPa Show Supplier Material materials with Elastic modulus of 7.8 GPa | dry | ISO 527-1/-2 | |
150 °C | 5.1 GPa Show Supplier Material materials with Elastic modulus of 5.1 GPa | dry | ISO 527-1/-2 | |
160 °C | 4.8 GPa Show Supplier Material materials with Elastic modulus of 4.8 GPa | dry | ISO 527-1/-2 | |
180 °C | 4.4 GPa Show Supplier Material materials with Elastic modulus of 4.4 GPa | dry | ISO 527-1/-2 | |
200 °C | 4.2 GPa Show Supplier Material materials with Elastic modulus of 4.2 GPa | dry | ISO 527-1/-2 | |
210 °C | 4 GPa Show Supplier Material materials with Elastic modulus of 4 GPa | dry | ISO 527-1/-2 | |
Elongation | -40 °C | 1.9 % Show Supplier Material materials with Elongation of 1.9 % | conditioned | ISO 527-1/-2 |
-40 °C | 2.2 % Show Supplier Material materials with Elongation of 2.2 % | dry | ISO 527-1/-2 | |
1.9 % Show Supplier Material materials with Elongation of 1.9 % | conditioned | ISO 527-1/-2 | ||
2.1 % Show Supplier Material materials with Elongation of 2.1 % | dry | ISO 527-1/-2 | ||
40 °C | 2 % Show Supplier Material materials with Elongation of 2 % | conditioned | ISO 527-1/-2 | |
40 °C | 2.3 % Show Supplier Material materials with Elongation of 2.3 % | dry | ISO 527-1/-2 | |
80 °C | 2.7 % Show Supplier Material materials with Elongation of 2.7 % | dry | ISO 527-1/-2 | |
80 °C | 5 % Show Supplier Material materials with Elongation of 5 % | conditioned | ISO 527-1/-2 | |
100 °C | 3.3 % Show Supplier Material materials with Elongation of 3.3 % | dry | ISO 527-1/-2 | |
100 °C | 5.5 % Show Supplier Material materials with Elongation of 5.5 % | conditioned | ISO 527-1/-2 | |
120 °C | 5 % Show Supplier Material materials with Elongation of 5 % | dry | ISO 527-1/-2 | |
120 °C | 6.5 % Show Supplier Material materials with Elongation of 6.5 % | conditioned | ISO 527-1/-2 | |
150 °C | 7.5 % Show Supplier Material materials with Elongation of 7.5 % | dry | ISO 527-1/-2 | |
160 °C | 8 % Show Supplier Material materials with Elongation of 8 % | dry | ISO 527-1/-2 | |
180 °C | 8 % Show Supplier Material materials with Elongation of 8 % | dry | ISO 527-1/-2 | |
200 °C | 8 % Show Supplier Material materials with Elongation of 8 % | dry | ISO 527-1/-2 | |
210 °C | 0.008 % Show Supplier Material materials with Elongation of 0.008 % | dry | ISO 527-1/-2 | |
Flexural modulus | 10.6 GPa Show Supplier Material materials with Flexural modulus of 10.6 GPa | dry | ISO 178 | |
11.2 GPa Show Supplier Material materials with Flexural modulus of 11.2 GPa | conditioned | ISO 178 | ||
120 °C | 7.7 GPa Show Supplier Material materials with Flexural modulus of 7.7 GPa | dry | ISO 178 | |
160 °C | 4.6 GPa Show Supplier Material materials with Flexural modulus of 4.6 GPa | dry | ISO 178 | |
180 °C | 4 GPa Show Supplier Material materials with Flexural modulus of 4 GPa | dry | ISO 178 | |
200 °C | 3.8 GPa Show Supplier Material materials with Flexural modulus of 3.8 GPa | dry | ISO 178 | |
210 °C | 3.7 GPa Show Supplier Material materials with Flexural modulus of 3.7 GPa | dry | ISO 178 | |
Flexural yield strength | 230 MPa Show Supplier Material materials with Flexural yield strength of 230 MPa | conditioned | ISO 178 | |
290 MPa Show Supplier Material materials with Flexural yield strength of 290 MPa | dry | ISO 178 | ||
120 °C | 170 MPa Show Supplier Material materials with Flexural yield strength of 170 MPa | dry | ISO 178 | |
160 °C | 110 MPa Show Supplier Material materials with Flexural yield strength of 110 MPa | dry | ISO 178 | |
180 °C | 100 MPa Show Supplier Material materials with Flexural yield strength of 100 MPa | dry | ISO 178 | |
200 °C | 90 MPa Show Supplier Material materials with Flexural yield strength of 90 MPa | dry | ISO 178 | |
210 °C | 85 MPa Show Supplier Material materials with Flexural yield strength of 85 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | -30 °C | 8 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 8 kJ/m² | conditioned | ISO 179/1eA |
-30 °C | 9 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 9 kJ/m² | dry | ISO 179/1eA | |
23 °C | 8 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 8 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 9 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 9 kJ/m² | dry | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 40 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 40 kJ/m² | conditioned | ISO 179/1eU |
-30 °C | 45 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 45 kJ/m² | dry | ISO 179/1eU | |
23 °C | 45 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 45 kJ/m² | conditioned | ISO 179/1eU | |
23 °C | 55.0 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 55.0 kJ/m² | dry | ISO 179/1eU | |
Tensile strength | -40 °C | 190 MPa Show Supplier Material materials with Tensile strength of 190 MPa | conditioned | ISO 527-1/-2 |
-40 °C | 210 MPa Show Supplier Material materials with Tensile strength of 210 MPa | dry | ISO 527-1/-2 | |
170 MPa Show Supplier Material materials with Tensile strength of 170 MPa | conditioned | ISO 527-1/-2 | ||
190 MPa Show Supplier Material materials with Tensile strength of 190 MPa | dry | ISO 527-1/-2 | ||
40 °C | 160 MPa Show Supplier Material materials with Tensile strength of 160 MPa | conditioned | ISO 527-1/-2 | |
40 °C | 190 MPa Show Supplier Material materials with Tensile strength of 190 MPa | dry | ISO 527-1/-2 | |
80 °C | 90 MPa Show Supplier Material materials with Tensile strength of 90 MPa | conditioned | ISO 527-1/-2 | |
80 °C | 180 MPa Show Supplier Material materials with Tensile strength of 180 MPa | dry | ISO 527-1/-2 | |
100 °C | 75 MPa Show Supplier Material materials with Tensile strength of 75 MPa | conditioned | ISO 527-1/-2 | |
100 °C | 160 MPa Show Supplier Material materials with Tensile strength of 160 MPa | dry | ISO 527-1/-2 | |
120 °C | 130 MPa Show Supplier Material materials with Tensile strength of 130 MPa | dry | ISO 527-1/-2 | |
150 °C | 95 MPa Show Supplier Material materials with Tensile strength of 95 MPa | dry | ISO 527-1/-2 | |
160 °C | 90 MPa Show Supplier Material materials with Tensile strength of 90 MPa | dry | ISO 527-1/-2 | |
180 °C | 80 MPa Show Supplier Material materials with Tensile strength of 80 MPa | dry | ISO 527-1/-2 | |
200 °C | 74 MPa Show Supplier Material materials with Tensile strength of 74 MPa | dry | ISO 527-1/-2 | |
210 °C | 70 MPa Show Supplier Material materials with Tensile strength of 70 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 3.3e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 3.3e-07 1/K | dry | ASTM D696 | Parallel | |
4e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 4e-07 1/K | dry | ASTM D696 | Normal | ||
Glass transition temperature | 125 °C Show Supplier Material materials with Glass transition temperature of 125 °C | dry | ISO 11357-1/-2 | 10°C/min | |
130 °C Show Supplier Material materials with Glass transition temperature of 130 °C | dry | ASTM D5026/D7028 | DMTA (tan d) | ||
Heat deflection temperature | 303 °C Show Supplier Material materials with Heat deflection temperature of 303 °C | dry | ISO 75-1/-2 | 2 MPa | |
316 °C Show Supplier Material materials with Heat deflection temperature of 316 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Melting point | 325 °C Show Supplier Material materials with Melting point of 325 °C | dry | ISO 11357-1/-3 | 10°C/min |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 375 V Show Supplier Material materials with Comparative tracking index of 375 V | dry | IEC 60112 | |
Dielectric constant | 4.4 [-] Show Supplier Material materials with Dielectric constant of 4.4 [-] | dry | IEC 62631-2-1 | 1MHz |
4.6 [-] Show Supplier Material materials with Dielectric constant of 4.6 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
4.7 [-] Show Supplier Material materials with Dielectric constant of 4.7 [-] | dry | IEC 62631-2-1 | 100Hz | |
5.6 [-] Show Supplier Material materials with Dielectric constant of 5.6 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Dissipation factor | 61 [-] Show Supplier Material materials with Dissipation factor of 61 [-] | dry | IEC 62631-2-1 | 100Hz |
200 [-] Show Supplier Material materials with Dissipation factor of 200 [-] | dry | IEC 62631-2-1 | 1MHz | |
260 [-] Show Supplier Material materials with Dissipation factor of 260 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
310 [-] Show Supplier Material materials with Dissipation factor of 310 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry, conditioned | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Crankshaft Covers | |
Fillers | 30% Glass Fiber |