General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.49 g/cm³ Show Supplier Material materials with Density of 1.49 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 2.3 % Show Supplier Material materials with Moisture absorption of 2.3 % | dry | Sim. to ISO 62 | |
Water absorption | 1.8 % Show Supplier Material materials with Water absorption of 1.8 % | dry | ISO 62 | at 23°C after 24h |
6.7 % Show Supplier Material materials with Water absorption of 6.7 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 8 GPa Show Supplier Material materials with Elastic modulus of 8 GPa | conditioned | ISO 527-1/-2 | |||
12.5 GPa Show Supplier Material materials with Elastic modulus of 12.5 GPa | dry | ISO 527-1/-2 | 1 mm | |||
12.5 GPa Show Supplier Material materials with Elastic modulus of 12.5 GPa | dry | ISO 527-1/-2 | 1 mm | |||
Elongation | 2.5 % Show Supplier Material materials with Elongation of 2.5 % | dry | ISO 527-1/-2 | 1 mm | ||
2.6 % Show Supplier Material materials with Elongation of 2.6 % | dry | ISO 527-1/-2 | 1 mm | |||
3.6 % Show Supplier Material materials with Elongation of 3.6 % | conditioned | ISO 527-1/-2 | ||||
Flexural modulus | 8 GPa Show Supplier Material materials with Flexural modulus of 8 GPa | conditioned | ISO 178 | |||
12.5 GPa Show Supplier Material materials with Flexural modulus of 12.5 GPa | dry | ISO 178 | ||||
Impact strength, Charpy notched | 23 °C | 12 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 12 kJ/m² | dry | ISO 179/1eA | ||
23 °C | 13 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 13 kJ/m² | conditioned | ISO 179/1eA | |||
Impact strength, Charpy unnotched | 23 °C | 60 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 60 kJ/m² | dry | ISO 179/1eU | ||
23 °C | 70 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 70 kJ/m² | conditioned | ISO 179/1eU | |||
Tensile strength | 140 MPa Show Supplier Material materials with Tensile strength of 140 MPa | conditioned | ISO 527-1/-2 | |||
200 MPa Show Supplier Material materials with Tensile strength of 200 MPa | dry | ISO 527-1/-2 | 1 mm | |||
210 MPa Show Supplier Material materials with Tensile strength of 210 MPa | dry | ISO 527-1/-2 | 1 mm | at low thickness |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Thickness | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 3.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 3.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
4e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 4e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Glass transition temperature | 75 °C Show Supplier Material materials with Glass transition temperature of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Heat deflection temperature | 290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 2 MPa | ||
290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 295 °C Show Supplier Material materials with Melting point of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 0.75 mm |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 425 V Show Supplier Material materials with Comparative tracking index of 425 V | dry | IEC 60112 | |
Dielectric constant | 4.4 [-] Show Supplier Material materials with Dielectric constant of 4.4 [-] | dry | IEC 62631-2-1 | 1MHz |
4.8 [-] Show Supplier Material materials with Dielectric constant of 4.8 [-] | dry | IEC 62631-2-1 | 100Hz | |
5.2 [-] Show Supplier Material materials with Dielectric constant of 5.2 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
11.2 [-] Show Supplier Material materials with Dielectric constant of 11.2 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Dielectric strength | 30 kV/mm Show Supplier Material materials with Dielectric strength of 30 kV/mm | conditioned | IEC 60243-1 | |
33 kV/mm Show Supplier Material materials with Dielectric strength of 33 kV/mm | dry | IEC 60243-1 | ||
Dissipation factor | 80 [-] Show Supplier Material materials with Dissipation factor of 80 [-] | dry | IEC 62631-2-1 | 100Hz |
170 [-] Show Supplier Material materials with Dissipation factor of 170 [-] | dry | IEC 62631-2-1 | 1MHz | |
850 [-] Show Supplier Material materials with Dissipation factor of 850 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
1400 [-] Show Supplier Material materials with Dissipation factor of 1400 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+11 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+11 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Reflow connectors (2) | |
Certifications | Yellow Card Available | |
Fillers | 35% Glass Fiber |