General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.45 g/cm³ Show Supplier Material materials with Density of 1.45 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.4 % Show Supplier Material materials with Moisture absorption of 1.4 % | dry | Sim. to ISO 62 |
Water absorption | 3.9 % Show Supplier Material materials with Water absorption of 3.9 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | -40 °C | 12 GPa Show Supplier Material materials with Elastic modulus of 12 GPa | dry | ISO 527-1/-2 |
11 GPa Show Supplier Material materials with Elastic modulus of 11 GPa | conditioned | ISO 527-1/-2 | ||
11.5 GPa Show Supplier Material materials with Elastic modulus of 11.5 GPa | dry | ISO 527-1/-2 | ||
80 °C | 9 GPa Show Supplier Material materials with Elastic modulus of 9 GPa | dry | ISO 527-1/-2 | |
100 °C | 7 GPa Show Supplier Material materials with Elastic modulus of 7 GPa | dry | ISO 527-1/-2 | |
120 °C | 5.5 GPa Show Supplier Material materials with Elastic modulus of 5.5 GPa | dry | ISO 527-1/-2 | |
140 °C | 4.7 GPa Show Supplier Material materials with Elastic modulus of 4.7 GPa | dry | ISO 527-1/-2 | |
160 °C | 4.2 GPa Show Supplier Material materials with Elastic modulus of 4.2 GPa | dry | ISO 527-1/-2 | |
Elongation | -40 °C | 2.4 % Show Supplier Material materials with Elongation of 2.4 % | dry | ISO 527-1/-2 |
2.3 % Show Supplier Material materials with Elongation of 2.3 % | dry | ISO 527-1/-2 | ||
2.4 % Show Supplier Material materials with Elongation of 2.4 % | conditioned | ISO 527-1/-2 | ||
80 °C | 2.8 % Show Supplier Material materials with Elongation of 2.8 % | dry | ISO 527-1/-2 | |
100 °C | 3.8 % Show Supplier Material materials with Elongation of 3.8 % | dry | ISO 527-1/-2 | |
120 °C | 4.5 % Show Supplier Material materials with Elongation of 4.5 % | dry | ISO 527-1/-2 | |
140 °C | 4.5 % Show Supplier Material materials with Elongation of 4.5 % | dry | ISO 527-1/-2 | |
160 °C | 4.5 % Show Supplier Material materials with Elongation of 4.5 % | dry | ISO 527-1/-2 | |
Flexural modulus | 10 GPa Show Supplier Material materials with Flexural modulus of 10 GPa | dry | ISO 178 | |
Flexural yield strength | 230 MPa Show Supplier Material materials with Flexural yield strength of 230 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | 23 °C | 8 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 8 kJ/m² | dry, conditioned | ISO 179/1eA |
Impact strength, Charpy unnotched | 23 °C | 55.0 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 55.0 kJ/m² | dry | ISO 179/1eU |
Tensile strength | -40 °C | 180 MPa Show Supplier Material materials with Tensile strength of 180 MPa | dry | ISO 527-1/-2 |
145 MPa Show Supplier Material materials with Tensile strength of 145 MPa | conditioned | ISO 527-1/-2 | ||
155 MPa Show Supplier Material materials with Tensile strength of 155 MPa | dry | ISO 527-1/-2 | ||
80 °C | 110 MPa Show Supplier Material materials with Tensile strength of 110 MPa | dry | ISO 527-1/-2 | |
100 °C | 85 MPa Show Supplier Material materials with Tensile strength of 85 MPa | dry | ISO 527-1/-2 | |
120 °C | 70 MPa Show Supplier Material materials with Tensile strength of 70 MPa | dry | ISO 527-1/-2 | |
140 °C | 60 MPa Show Supplier Material materials with Tensile strength of 60 MPa | dry | ISO 527-1/-2 | |
160 °C | 55.0 MPa Show Supplier Material materials with Tensile strength of 55.0 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 2e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
7e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 7e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Flammability | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 0.4 mm | |||
Heat deflection temperature | 275 °C Show Supplier Material materials with Heat deflection temperature of 275 °C | dry | ISO 75-1/-2 | 2 MPa | ||
300 °C Show Supplier Material materials with Heat deflection temperature of 300 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 325 °C Show Supplier Material materials with Melting point of 325 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 150 °C Show Supplier Material materials with Relative temperature index, electrical of 150 °C | dry | UL746B | 0.75 mm | ||
Thermal conductivity | 0.35 W/(m·K) Show Supplier Material materials with Thermal conductivity of 0.35 W/(m·K) | dry | ASTM E1461 | through plane | ||
0.41 W/(m·K) Show Supplier Material materials with Thermal conductivity of 0.41 W/(m·K) | dry | ASTM E1461 | in plane |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 600 V Show Supplier Material materials with Comparative tracking index of 600 V | dry | IEC 60112 | |
Dielectric constant | 3.6 [-] Show Supplier Material materials with Dielectric constant of 3.6 [-] | dry | IEC 60250 | 10GHz |
3.7 [-] Show Supplier Material materials with Dielectric constant of 3.7 [-] | dry | IEC 60250 | 1GHz | |
3.75 [-] Show Supplier Material materials with Dielectric constant of 3.75 [-] | conditioned | IEC 60250 | 10GHz | |
3.9 [-] Show Supplier Material materials with Dielectric constant of 3.9 [-] | conditioned | IEC 60250 | 1GHz | |
Dielectric strength | 33 kV/mm Show Supplier Material materials with Dielectric strength of 33 kV/mm | dry | IEC 60243-1 | |
Dissipation factor | 100 [-] Show Supplier Material materials with Dissipation factor of 100 [-] | dry | IEC 60250 | 10GHz |
140 [-] Show Supplier Material materials with Dissipation factor of 140 [-] | dry | IEC 60250 | 1GHz | |
150 [-] Show Supplier Material materials with Dissipation factor of 150 [-] | conditioned | IEC 60250 | 10GHz | |
200 [-] Show Supplier Material materials with Dissipation factor of 200 [-] | conditioned | IEC 60250 | 1GHz | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry, conditioned | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Reflow connectors, DDR DIMM Connectors, Audio Jack Connectors, Reflow connectors (2), Reflow connectors (3) | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber |