General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.52 g/cm³ Show Supplier Material materials with Density of 1.52 g/cm³ | dry | ISO 1183 |
Limiting oxygen index | 20 % Show Supplier Material materials with Limiting oxygen index of 20 % | dry | ISO 4589-1/-2 |
Moisture absorption | 0.15 % Show Supplier Material materials with Moisture absorption of 0.15 % | dry | Sim. to ISO 62 |
Water absorption | 0.3 % Show Supplier Material materials with Water absorption of 0.3 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | -40 °C | 11 GPa Show Supplier Material materials with Elastic modulus of 11 GPa | dry | ISO 527-1/-2 |
9.3 GPa Show Supplier Material materials with Elastic modulus of 9.3 GPa | dry | ISO 527-1/-2 | ||
100 °C | 4.4 GPa Show Supplier Material materials with Elastic modulus of 4.4 GPa | dry | ISO 527-1/-2 | |
120 °C | 4 GPa Show Supplier Material materials with Elastic modulus of 4 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.1 GPa Show Supplier Material materials with Elastic modulus of 3.1 GPa | dry | ISO 527-1/-2 | |
180 °C | 2.7 GPa Show Supplier Material materials with Elastic modulus of 2.7 GPa | dry | ISO 527-1/-2 | |
Elongation | -40 °C | 2.8 % Show Supplier Material materials with Elongation of 2.8 % | dry | ISO 527-1/-2 |
3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | ||
120 °C | 5.7 % Show Supplier Material materials with Elongation of 5.7 % | dry | ISO 527-1/-2 | |
160 °C | 6 % Show Supplier Material materials with Elongation of 6 % | dry | ISO 527-1/-2 | |
180 °C | 6 % Show Supplier Material materials with Elongation of 6 % | dry | ISO 527-1/-2 | |
Flexural modulus | 9 GPa Show Supplier Material materials with Flexural modulus of 9 GPa | dry | ISO 178 | |
120 °C | 4 GPa Show Supplier Material materials with Flexural modulus of 4 GPa | dry | ISO 178 | |
160 °C | 3.2 GPa Show Supplier Material materials with Flexural modulus of 3.2 GPa | dry | ISO 178 | |
Flexural yield strength | 205 MPa Show Supplier Material materials with Flexural yield strength of 205 MPa | dry | ISO 178 | |
120 °C | 95 MPa Show Supplier Material materials with Flexural yield strength of 95 MPa | dry | ISO 178 | |
160 °C | 70 MPa Show Supplier Material materials with Flexural yield strength of 70 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | -30 °C | 8 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 8 kJ/m² | dry | ISO 179/1eA |
23 °C | 8 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 8 kJ/m² | dry | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 45 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 45 kJ/m² | dry | ISO 179/1eU |
23 °C | 60 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 60 kJ/m² | dry | ISO 179/1eU | |
Tensile strength | -40 °C | 200 MPa Show Supplier Material materials with Tensile strength of 200 MPa | dry | ISO 527-1/-2 |
130 MPa Show Supplier Material materials with Tensile strength of 130 MPa | dry | ISO 527-1/-2 | ||
100 °C | 72 MPa Show Supplier Material materials with Tensile strength of 72 MPa | dry | ISO 527-1/-2 | |
120 °C | 64 MPa Show Supplier Material materials with Tensile strength of 64 MPa | dry | ISO 527-1/-2 | |
160 °C | 50 MPa Show Supplier Material materials with Tensile strength of 50 MPa | dry | ISO 527-1/-2 | |
180 °C | 40 MPa Show Supplier Material materials with Tensile strength of 40 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 2.7e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2.7e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
6.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 6.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Heat deflection temperature | 205 °C Show Supplier Material materials with Heat deflection temperature of 205 °C | dry | ISO 75-1/-2 | 2 MPa | |
220 °C Show Supplier Material materials with Heat deflection temperature of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Melting point | 225 °C Show Supplier Material materials with Melting point of 225 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Thermal diffusivity | 8.23e-08 mm²/s Show Supplier Material materials with Thermal diffusivity of 8.23e-08 mm²/s | dry | - |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 350 V Show Supplier Material materials with Comparative tracking index of 350 V | dry | IEC 60112 | |
Dielectric constant | 3.7 [-] Show Supplier Material materials with Dielectric constant of 3.7 [-] | dry | IEC 62631-2-1 | 1MHz |
3.9 [-] Show Supplier Material materials with Dielectric constant of 3.9 [-] | dry | IEC 62631-2-1 | 100Hz | |
Dielectric strength | 30 kV/mm Show Supplier Material materials with Dielectric strength of 30 kV/mm | dry | IEC 60243-1 | |
Dissipation factor | 25 [-] Show Supplier Material materials with Dissipation factor of 25 [-] | dry | IEC 62631-2-1 | 100Hz |
170 [-] Show Supplier Material materials with Dissipation factor of 170 [-] | dry | IEC 62631-2-1 | 1MHz | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Density of melt | 1220 g/cm³ Show Supplier Material materials with Density of melt of 1220 g/cm³ | dry | - | ||
Melt volume-flow rate | 250 °C | 14.0 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 14.0 cm³/10min | dry | ISO 1133 | |
Shrinkage | 0.33 % Show Supplier Material materials with Shrinkage of 0.33 % | dry | Sim. to ISO 294-4 | Parallel | |
1.2 % Show Supplier Material materials with Shrinkage of 1.2 % | dry | Sim. to ISO 294-4 | Normal | ||
Specific heat capacity melt | 1850 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1850 J/(kg·K) | dry | - | ||
Thermal conductivity of melt | 0.185 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.185 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Sensors PBT HR, Connectors PBT HR, Control Devices PBT HR | |
Fillers | 30% Glass Fiber |