General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.43 g/cm³ Show Supplier Material materials with Density of 1.43 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 1.6 % Show Supplier Material materials with Moisture absorption of 1.6 % | dry | Sim. to ISO 62 | |
Water absorption | 1 % Show Supplier Material materials with Water absorption of 1 % | dry | ISO 62 | at 23°C after 24h |
4.9 % Show Supplier Material materials with Water absorption of 4.9 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Elastic modulus | -40 °C | 1.1 GPa Show Supplier Material materials with Elastic modulus of 1.1 GPa | dry | ISO 527-1/-2 | ||
7.9 GPa Show Supplier Material materials with Elastic modulus of 7.9 GPa | conditioned | ISO 527-1/-2 | ||||
8.6 GPa Show Supplier Material materials with Elastic modulus of 8.6 GPa | conditioned | ISO 527-1/-2 | ||||
11 GPa Show Supplier Material materials with Elastic modulus of 11 GPa | dry | ISO 527-1/-2 | ||||
11.5 GPa Show Supplier Material materials with Elastic modulus of 11.5 GPa | dry | ISO 527-1/-2 | 1 mm | |||
100 °C | 5.8 GPa Show Supplier Material materials with Elastic modulus of 5.8 GPa | dry | ISO 527-1/-2 | |||
120 °C | 5.3 GPa Show Supplier Material materials with Elastic modulus of 5.3 GPa | dry | ISO 527-1/-2 | |||
140 °C | 4.8 GPa Show Supplier Material materials with Elastic modulus of 4.8 GPa | dry | ISO 527-1/-2 | |||
160 °C | 4.6 GPa Show Supplier Material materials with Elastic modulus of 4.6 GPa | dry | ISO 527-1/-2 | |||
Elongation | -40 °C | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | ||
2.7 % Show Supplier Material materials with Elongation of 2.7 % | dry | ISO 527-1/-2 | 1 mm | |||
3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | ||||
3.4 % Show Supplier Material materials with Elongation of 3.4 % | conditioned | ISO 527-1/-2 | ||||
4.3 % Show Supplier Material materials with Elongation of 4.3 % | conditioned | ISO 527-1/-2 | ||||
120 °C | 5.4 % Show Supplier Material materials with Elongation of 5.4 % | dry | ISO 527-1/-2 | |||
140 °C | 5.7 % Show Supplier Material materials with Elongation of 5.7 % | dry | ISO 527-1/-2 | |||
160 °C | 6 % Show Supplier Material materials with Elongation of 6 % | dry | ISO 527-1/-2 | |||
Flexural modulus | 7.5 GPa Show Supplier Material materials with Flexural modulus of 7.5 GPa | conditioned | ISO 178 | |||
11.5 GPa Show Supplier Material materials with Flexural modulus of 11.5 GPa | dry | ISO 178 | ||||
120 °C | 5.8 GPa Show Supplier Material materials with Flexural modulus of 5.8 GPa | dry | ISO 178 | |||
160 °C | 5.0 GPa Show Supplier Material materials with Flexural modulus of 5.0 GPa | dry | ISO 178 | |||
Flexural yield strength | 180 MPa Show Supplier Material materials with Flexural yield strength of 180 MPa | conditioned | ISO 178 | |||
240 MPa Show Supplier Material materials with Flexural yield strength of 240 MPa | dry | ISO 178 | ||||
120 °C | 120 MPa Show Supplier Material materials with Flexural yield strength of 120 MPa | dry | ISO 178 | |||
160 °C | 100 MPa Show Supplier Material materials with Flexural yield strength of 100 MPa | dry | ISO 178 | |||
Impact strength, Charpy notched | -30 °C | 10 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 10 kJ/m² | dry, conditioned | ISO 179/1eA | ||
23 °C | 10 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 10 kJ/m² | dry, conditioned | ISO 179/1eA | |||
Impact strength, Charpy unnotched | -30 °C | 48 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 48 kJ/m² | conditioned | ISO 179/1eU | ||
-30 °C | 50 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 50 kJ/m² | dry | ISO 179/1eU | |||
23 °C | 62 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 62 kJ/m² | conditioned | ISO 179/1eU | |||
23 °C | 68 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 68 kJ/m² | dry | ISO 179/1eU | |||
Tensile strength | -40 °C | 200 MPa Show Supplier Material materials with Tensile strength of 200 MPa | dry | ISO 527-1/-2 | ||
100 MPa Show Supplier Material materials with Tensile strength of 100 MPa | conditioned | ISO 527-1/-2 | at low thickness | |||
120 MPa Show Supplier Material materials with Tensile strength of 120 MPa | conditioned | ISO 527-1/-2 | ||||
145 MPa Show Supplier Material materials with Tensile strength of 145 MPa | dry | ISO 527-1/-2 | 1 mm | at low thickness | ||
155 MPa Show Supplier Material materials with Tensile strength of 155 MPa | dry | ISO 527-1/-2 | ||||
100 °C | 87 MPa Show Supplier Material materials with Tensile strength of 87 MPa | dry | ISO 527-1/-2 | |||
120 °C | 79 MPa Show Supplier Material materials with Tensile strength of 79 MPa | dry | ISO 527-1/-2 | |||
140 °C | 72 MPa Show Supplier Material materials with Tensile strength of 72 MPa | dry | ISO 527-1/-2 | |||
160 °C | 66 MPa Show Supplier Material materials with Tensile strength of 66 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Ball pressure temperature | 255 °C Show Supplier Material materials with Ball pressure temperature of 255 °C | dry | IEC 60695-10-2 | |||
Coefficient of thermal expansion | 2.1e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2.1e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
6.7e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 6.7e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Flammability | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Glass transition temperature | 60 °C Show Supplier Material materials with Glass transition temperature of 60 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 0.4 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | |||
Glow Wire Ignition Temperature | 800 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 800 °C | dry | IEC 60695-2-13 | 0.4 mm | ||
825 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 825 °C | dry | IEC 60695-2-13 | 3 mm | |||
Heat deflection temperature | 247 °C Show Supplier Material materials with Heat deflection temperature of 247 °C | dry | ISO 75-1/-2 | 2 MPa | ||
Melting point | 260 °C Show Supplier Material materials with Melting point of 260 °C | dry | ISO 11357-1/-3 | 10°C/min |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 600 V Show Supplier Material materials with Comparative tracking index of 600 V | dry | IEC 60112 | |
700 V Show Supplier Material materials with Comparative tracking index of 700 V | dry | Sim. to IEC 60112 | Above 600V | |
Dielectric constant | 3.6 [-] Show Supplier Material materials with Dielectric constant of 3.6 [-] | dry | IEC 60250 | 1GHz |
3.7 [-] Show Supplier Material materials with Dielectric constant of 3.7 [-] | conditioned | IEC 60250 | 1GHz | |
3.9 [-] Show Supplier Material materials with Dielectric constant of 3.9 [-] | dry | IEC 62631-2-1 | 1MHz | |
4.2 [-] Show Supplier Material materials with Dielectric constant of 4.2 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.3 [-] Show Supplier Material materials with Dielectric constant of 4.3 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
7.3 [-] Show Supplier Material materials with Dielectric constant of 7.3 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Dielectric strength | 38 kV/mm Show Supplier Material materials with Dielectric strength of 38 kV/mm | conditioned | IEC 60243-1 | |
41 kV/mm Show Supplier Material materials with Dielectric strength of 41 kV/mm | dry | IEC 60243-1 | ||
Dissipation factor | 100 [-] Show Supplier Material materials with Dissipation factor of 100 [-] | dry | IEC 60250 | 1GHz |
110 [-] Show Supplier Material materials with Dissipation factor of 110 [-] | dry, conditioned | IEC 62631-2-1 | 100Hz | |
140 [-] Show Supplier Material materials with Dissipation factor of 140 [-] | conditioned | IEC 60250 | 1GHz | |
150 [-] Show Supplier Material materials with Dissipation factor of 150 [-] | dry | IEC 62631-2-1 | 1MHz | |
490 [-] Show Supplier Material materials with Dissipation factor of 490 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
Surface resistivity | 3e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 3e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | dry | IEC 62631-3-2 | ||
Volume resistivity | 5e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 5e+12 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Shrinkage | 0.28 % Show Supplier Material materials with Shrinkage of 0.28 % | dry | ISO 294-4 | Parallel |
1.31 % Show Supplier Material materials with Shrinkage of 1.31 % | dry | ISO 294-4 | Normal | |
Spiral flow length | 87 | dry | - | 1.0 mm 800 bar |
104 | dry | - | 1.0 mm 1000 bar | |
121 | dry | - | 1.0 mm 1200 bar |
Technological properties
Property | ||
---|---|---|
Application areas | High voltage connector e-motor, High voltage connector, EV Charging Plugs | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber |