General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.67 g/cm³ Show Supplier Material materials with Density of 1.67 g/cm³ | dry | ISO 1183 | |
Limiting oxygen index | 37 % Show Supplier Material materials with Limiting oxygen index of 37 % | dry | ISO 4589-1/-2 | |
Moisture absorption | 1.8 % Show Supplier Material materials with Moisture absorption of 1.8 % | dry | Sim. to ISO 62 | |
Water absorption | 1.7 % Show Supplier Material materials with Water absorption of 1.7 % | dry | ISO 62 | at 23°C after 24h |
5.9 % Show Supplier Material materials with Water absorption of 5.9 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Thickness | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 8 GPa Show Supplier Material materials with Elastic modulus of 8 GPa | conditioned | ISO 527-1/-2 | |||
12 GPa Show Supplier Material materials with Elastic modulus of 12 GPa | dry | ISO 527-1/-2 | ||||
12 GPa Show Supplier Material materials with Elastic modulus of 12 GPa | dry | ISO 527-1/-2 | 1 mm | |||
120 °C | 7.5 GPa Show Supplier Material materials with Elastic modulus of 7.5 GPa | dry | ISO 527-1/-2 | |||
160 °C | 6.2 GPa Show Supplier Material materials with Elastic modulus of 6.2 GPa | dry | ISO 527-1/-2 | |||
Elongation | 2.4 % Show Supplier Material materials with Elongation of 2.4 % | dry | ISO 527-1/-2 | |||
2.4 % Show Supplier Material materials with Elongation of 2.4 % | dry | ISO 527-1/-2 | 1 mm | |||
3.5 % Show Supplier Material materials with Elongation of 3.5 % | conditioned | ISO 527-1/-2 | ||||
120 °C | 4 % Show Supplier Material materials with Elongation of 4 % | dry | ISO 527-1/-2 | |||
160 °C | 4 % Show Supplier Material materials with Elongation of 4 % | dry | ISO 527-1/-2 | |||
Flexural modulus | 7.3 GPa Show Supplier Material materials with Flexural modulus of 7.3 GPa | conditioned | ISO 178 | |||
11 GPa Show Supplier Material materials with Flexural modulus of 11 GPa | dry | ISO 178 | ||||
120 °C | 6.5 GPa Show Supplier Material materials with Flexural modulus of 6.5 GPa | dry | ISO 178 | |||
160 °C | 5 GPa Show Supplier Material materials with Flexural modulus of 5 GPa | dry | ISO 178 | |||
Flexural yield strength | 190 MPa Show Supplier Material materials with Flexural yield strength of 190 MPa | conditioned | ISO 178 | |||
260 MPa Show Supplier Material materials with Flexural yield strength of 260 MPa | dry | ISO 178 | ||||
120 °C | 170 MPa Show Supplier Material materials with Flexural yield strength of 170 MPa | dry | ISO 178 | |||
160 °C | 140 MPa Show Supplier Material materials with Flexural yield strength of 140 MPa | dry | ISO 178 | |||
Impact strength, Charpy notched | -30 °C | 10 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 10 kJ/m² | dry, conditioned | ISO 179/1eA | ||
23 °C | 11 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 11 kJ/m² | dry, conditioned | ISO 179/1eA | |||
Impact strength, Charpy unnotched | -30 °C | 50 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 50 kJ/m² | dry, conditioned | ISO 179/1eU | ||
23 °C | 60 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 60 kJ/m² | dry, conditioned | ISO 179/1eU | |||
Tensile strength | 120 MPa Show Supplier Material materials with Tensile strength of 120 MPa | conditioned | ISO 527-1/-2 | |||
180 MPa Show Supplier Material materials with Tensile strength of 180 MPa | dry | ISO 527-1/-2 | ||||
180 MPa Show Supplier Material materials with Tensile strength of 180 MPa | dry | ISO 527-1/-2 | 1 mm | at low thickness | ||
120 °C | 105 MPa Show Supplier Material materials with Tensile strength of 105 MPa | dry | ISO 527-1/-2 | |||
160 °C | 95 MPa Show Supplier Material materials with Tensile strength of 95 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 2.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
5.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 5.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Flammability | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Glass transition temperature | 75 °C Show Supplier Material materials with Glass transition temperature of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 0.75 mm | |||
Glow Wire Ignition Temperature | 800 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 800 °C | dry | IEC 60695-2-13 | 0.75 mm | ||
925 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 925 °C | dry | IEC 60695-2-13 | 3 mm | |||
Heat deflection temperature | 290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 2 MPa | ||
290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 295 °C Show Supplier Material materials with Melting point of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 140 °C Show Supplier Material materials with Relative temperature index, electrical of 140 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 120 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 120 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 130 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 130 °C | dry | UL746B | 0.75 mm | ||
Thermal diffusivity | 1.11e-07 mm²/s Show Supplier Material materials with Thermal diffusivity of 1.11e-07 mm²/s | dry | - | |||
Vicat softening temperature | 290 °C Show Supplier Material materials with Vicat softening temperature of 290 °C | dry | ISO 306 | 50°C/h 50N |
Electrical
Property | Value | Condition | Testing Standard |
---|---|---|---|
Comparative tracking index | 175 V Show Supplier Material materials with Comparative tracking index of 175 V | dry | IEC 60112 |
Dielectric strength | 30 kV/mm Show Supplier Material materials with Dielectric strength of 30 kV/mm | dry | IEC 60243-1 |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 |
Volume resistivity | 1e+06 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+06 Ω·cm | conditioned | IEC 62631-3-1 |
1e+12 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+12 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 1450 g/cm³ Show Supplier Material materials with Density of melt of 1450 g/cm³ | dry | - | |
Shrinkage | 0.4 % Show Supplier Material materials with Shrinkage of 0.4 % | dry | Sim. to ISO 294-4 | Parallel |
1.1 % Show Supplier Material materials with Shrinkage of 1.1 % | dry | Sim. to ISO 294-4 | Normal | |
Specific heat capacity melt | 1620 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 1620 J/(kg·K) | dry | - | |
Spiral flow length | 105 | dry | - | 1.0 mm 800 bar |
115 | dry | - | 1.0 mm 900 bar | |
125 | dry | - | 1.0 mm 1000 bar | |
36 | dry | - | 0.5mm 1200 bar | |
50 | dry | - | 0.5mm 1600 bar | |
74 | dry | - | 0.5mm 2000 bar | |
Thermal conductivity of melt | 0.26 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.26 W/(m·K) | dry | - | |
Viscosity number | 145 cm³/gr Show Supplier Material materials with Viscosity number of 145 cm³/gr | dry | ISO 307, 1157, 1628 |
Technological properties
Property | ||
---|---|---|
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber |