General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.23 g/cm³ Show Supplier Material materials with Density of 1.23 g/cm³ | dry | ISO 1183 | |
Moisture absorption | 3.2 % Show Supplier Material materials with Moisture absorption of 3.2 % | dry | Sim. to ISO 62 | |
Water absorption | 3.2 % Show Supplier Material materials with Water absorption of 3.2 % | dry | ISO 62 | at 23°C after 24h |
11.5 % Show Supplier Material materials with Water absorption of 11.5 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | -40 °C | 13 GPa Show Supplier Material materials with Elastic modulus of 13 GPa | dry | ISO 527-1/-2 |
7 GPa Show Supplier Material materials with Elastic modulus of 7 GPa | conditioned | ISO 527-1/-2 | ||
13 GPa Show Supplier Material materials with Elastic modulus of 13 GPa | dry | ISO 527-1/-2 | ||
120 °C | 6.8 GPa Show Supplier Material materials with Elastic modulus of 6.8 GPa | dry | ISO 527-1/-2 | |
160 °C | 6.4 GPa Show Supplier Material materials with Elastic modulus of 6.4 GPa | dry | ISO 527-1/-2 | |
180 °C | 6.1 GPa Show Supplier Material materials with Elastic modulus of 6.1 GPa | dry | ISO 527-1/-2 | |
200 °C | 5.2 GPa Show Supplier Material materials with Elastic modulus of 5.2 GPa | dry | ISO 527-1/-2 | |
Elongation | -40 °C | 2.2 % Show Supplier Material materials with Elongation of 2.2 % | dry | ISO 527-1/-2 |
2.3 % Show Supplier Material materials with Elongation of 2.3 % | dry | ISO 527-1/-2 | ||
4.3 % Show Supplier Material materials with Elongation of 4.3 % | conditioned | ISO 527-1/-2 | ||
120 °C | 3.3 % Show Supplier Material materials with Elongation of 3.3 % | dry | ISO 527-1/-2 | |
160 °C | 3.2 % Show Supplier Material materials with Elongation of 3.2 % | dry | ISO 527-1/-2 | |
180 °C | 3.2 % Show Supplier Material materials with Elongation of 3.2 % | dry | ISO 527-1/-2 | |
200 °C | 3.6 % Show Supplier Material materials with Elongation of 3.6 % | dry | ISO 527-1/-2 | |
Flexural modulus | 5.8 GPa Show Supplier Material materials with Flexural modulus of 5.8 GPa | conditioned | ISO 178 | |
11.5 GPa Show Supplier Material materials with Flexural modulus of 11.5 GPa | dry | ISO 178 | ||
120 °C | 5.8 GPa Show Supplier Material materials with Flexural modulus of 5.8 GPa | dry | ISO 178 | |
160 °C | 5.5 GPa Show Supplier Material materials with Flexural modulus of 5.5 GPa | dry | ISO 178 | |
Flexural yield strength | 150 MPa Show Supplier Material materials with Flexural yield strength of 150 MPa | conditioned | ISO 178 | |
290 MPa Show Supplier Material materials with Flexural yield strength of 290 MPa | dry | ISO 178 | ||
120 °C | 140 MPa Show Supplier Material materials with Flexural yield strength of 140 MPa | dry | ISO 178 | |
160 °C | 125 MPa Show Supplier Material materials with Flexural yield strength of 125 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | -30 °C | 4.5 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 4.5 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 5.5 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 5.5 kJ/m² | dry | ISO 179/1eA | |
23 °C | 12 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 12 kJ/m² | conditioned | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 40 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 40 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 45 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 45 kJ/m² | dry | ISO 179/1eU | |
23 °C | 70 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 70 kJ/m² | conditioned | ISO 179/1eU | |
Tensile strength | -40 °C | 250 MPa Show Supplier Material materials with Tensile strength of 250 MPa | dry | ISO 527-1/-2 |
130 MPa Show Supplier Material materials with Tensile strength of 130 MPa | conditioned | ISO 527-1/-2 | ||
210 MPa Show Supplier Material materials with Tensile strength of 210 MPa | dry | ISO 527-1/-2 | ||
120 °C | 100 MPa Show Supplier Material materials with Tensile strength of 100 MPa | dry | ISO 527-1/-2 | |
160 °C | 87 MPa Show Supplier Material materials with Tensile strength of 87 MPa | dry | ISO 527-1/-2 | |
180 °C | 81 MPa Show Supplier Material materials with Tensile strength of 81 MPa | dry | ISO 527-1/-2 | |
200 °C | 75 MPa Show Supplier Material materials with Tensile strength of 75 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 2.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Glass transition temperature | 75 °C Show Supplier Material materials with Glass transition temperature of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Heat deflection temperature | 290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 2 MPa | |
Melting point | 295 °C Show Supplier Material materials with Melting point of 295 °C | dry | ISO 11357-1/-3 | 10°C/min |
Electrical
Property | Value | Condition | Testing Standard |
---|---|---|---|
Volume resistivity | 100000 Ω·cm Show Supplier Material materials with Volume resistivity of 100000 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Oil Pump Gears (automotive), Power Lift Gate Actuators, Power Door Actuators, Power Window Actuators, Windshield Wiper Actuators, Power Seats, Gears | |
Fillers | 15% Carbon Fiber |