General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.43 g/cm³ Show Supplier Material materials with Density of 1.43 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.3 % Show Supplier Material materials with Moisture absorption of 1.3 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 8.8 GPa Show Supplier Material materials with Elastic modulus of 8.8 GPa | conditioned | ISO 527-1/-2 | |
12 GPa Show Supplier Material materials with Elastic modulus of 12 GPa | dry | ISO 527-1/-2 | ||
Elongation | 2.5 % Show Supplier Material materials with Elongation of 2.5 % | dry | ISO 527-1/-2 | |
3 % Show Supplier Material materials with Elongation of 3 % | conditioned | ISO 527-1/-2 | ||
Flexural modulus | 7.5 GPa Show Supplier Material materials with Flexural modulus of 7.5 GPa | conditioned | ISO 178 | |
10.2 GPa Show Supplier Material materials with Flexural modulus of 10.2 GPa | dry | ISO 178 | ||
Flexural yield strength | 160 MPa Show Supplier Material materials with Flexural yield strength of 160 MPa | conditioned | ISO 178 | |
220 MPa Show Supplier Material materials with Flexural yield strength of 220 MPa | dry | ISO 178 | ||
Impact strength, Charpy notched | 23 °C | 10 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 10 kJ/m² | dry | ISO 179/1eA |
23 °C | 16 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 16 kJ/m² | conditioned | ISO 179/1eA | |
Impact strength, Charpy unnotched | 23 °C | 63 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 63 kJ/m² | dry | ISO 179/1eU |
23 °C | 67 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 67 kJ/m² | conditioned | ISO 179/1eU | |
Tensile strength | 110 MPa Show Supplier Material materials with Tensile strength of 110 MPa | conditioned | ISO 527-1/-2 | |
140 MPa Show Supplier Material materials with Tensile strength of 140 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Thickness | Comment |
---|---|---|---|---|---|---|
Heat deflection temperature | 210 °C Show Supplier Material materials with Heat deflection temperature of 210 °C | dry | ISO 75-1/-2 | 2 MPa | ||
220 °C Show Supplier Material materials with Heat deflection temperature of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 220 °C Show Supplier Material materials with Melting point of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 0.75 mm |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 600 V Show Supplier Material materials with Comparative tracking index of 600 V | dry | IEC 60112 | |
Dielectric constant | 3.2 [-] Show Supplier Material materials with Dielectric constant of 3.2 [-] | dry | IEC 62631-2-1 | 1MHz |
Dielectric strength | 23 kV/mm Show Supplier Material materials with Dielectric strength of 23 kV/mm | dry | IEC 60243-1 | |
Dissipation factor | 200 [-] Show Supplier Material materials with Dissipation factor of 200 [-] | dry | IEC 62631-2-1 | 1MHz |
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Melt mass-flow rate | 270 °C | 13 g/10min Show Supplier Material materials with Melt mass-flow rate of 13 g/10min | dry | ISO 1133 | |
Melt volume-flow rate | 270 °C | 10 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 10 cm³/10min | dry | ISO 1133 | |
Shrinkage | 0.3 % Show Supplier Material materials with Shrinkage of 0.3 % | dry | ISO 294-4 | Parallel | |
0.8 % Show Supplier Material materials with Shrinkage of 0.8 % | dry | ISO 294-4 | Normal |
Technological properties
Property | ||
---|---|---|
Fillers | 30% Glass Fiber |