General
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density | 1.1 g/cm³ Show Supplier Material materials with Density of 1.1 g/cm³ | dry | ISO 1183 | |
Limiting oxygen index | 27 % Show Supplier Material materials with Limiting oxygen index of 27 % | dry | ISO 4589-1/-2 | |
Moisture absorption | 2.95 % Show Supplier Material materials with Moisture absorption of 2.95 % | dry | Sim. to ISO 62 | |
Water absorption | 3 % Show Supplier Material materials with Water absorption of 3 % | dry | ISO 62 | at 23°C after 24h |
11 % Show Supplier Material materials with Water absorption of 11 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 0.6 GPa Show Supplier Material materials with Elastic modulus of 0.6 GPa | conditioned | ISO 527-1/-2 | |
1.9 GPa Show Supplier Material materials with Elastic modulus of 1.9 GPa | dry | ISO 527-1/-2 | ||
120 °C | 0.4 GPa Show Supplier Material materials with Elastic modulus of 0.4 GPa | dry | ISO 527-1/-2 | |
160 °C | 0.35 GPa Show Supplier Material materials with Elastic modulus of 0.35 GPa | dry | ISO 527-1/-2 | |
Elongation | -40 °C | 66 % Show Supplier Material materials with Elongation of 66 % | dry | ISO 527-1/-2 |
50 % Show Supplier Material materials with Elongation of 50 % | dry, conditioned | ISO 527-1/-2 | ||
120 °C | 50 % Show Supplier Material materials with Elongation of 50 % | dry | ISO 527-1/-2 | |
160 °C | 50 % Show Supplier Material materials with Elongation of 50 % | dry | ISO 527-1/-2 | |
Elongation at yield | 20 % Show Supplier Material materials with Elongation at yield of 20 % | dry | ISO 527-1/-2 | |
25 % Show Supplier Material materials with Elongation at yield of 25 % | conditioned | ISO 527-1/-2 | ||
Flexural modulus | 0.55 GPa Show Supplier Material materials with Flexural modulus of 0.55 GPa | conditioned | ISO 178 | |
1.8 GPa Show Supplier Material materials with Flexural modulus of 1.8 GPa | dry | ISO 178 | ||
120 °C | 0.4 GPa Show Supplier Material materials with Flexural modulus of 0.4 GPa | dry | ISO 178 | |
160 °C | 0.35 GPa Show Supplier Material materials with Flexural modulus of 0.35 GPa | dry | ISO 178 | |
Flexural yield strength | 40 MPa Show Supplier Material materials with Flexural yield strength of 40 MPa | conditioned | ISO 178 | |
80 MPa Show Supplier Material materials with Flexural yield strength of 80 MPa | dry | ISO 178 | ||
120 °C | 40 MPa Show Supplier Material materials with Flexural yield strength of 40 MPa | dry | ISO 178 | |
160 °C | 30 MPa Show Supplier Material materials with Flexural yield strength of 30 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | -30 °C | 26 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 26 kJ/m² | dry | ISO 179/1eA |
-30 °C | 30 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 30 kJ/m² | conditioned | ISO 179/1eA | |
23 °C | 75 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 75 kJ/m² | dry | ISO 179/1eA | |
23 °C | 125 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 125 kJ/m² | conditioned | ISO 179/1eA | |
Tensile strength | -40 °C | 85 MPa Show Supplier Material materials with Tensile strength of 85 MPa | dry | ISO 527-1/-2 |
Yield strength | 45 MPa Show Supplier Material materials with Yield strength of 45 MPa | conditioned | ISO 527-1/-2 | |
60 MPa Show Supplier Material materials with Yield strength of 60 MPa | dry | ISO 527-1/-2 | ||
120 °C | 35 MPa Show Supplier Material materials with Yield strength of 35 MPa | dry | ISO 527-1/-2 | |
160 °C | 30 MPa Show Supplier Material materials with Yield strength of 30 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 1.6e-06 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.6e-06 1/K | dry | ISO 11359-1/-2 | Parallel | |
1.8e-06 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.8e-06 1/K | dry | ISO 11359-1/-2 | Normal | ||
Glass transition temperature | 75 °C Show Supplier Material materials with Glass transition temperature of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | |
Heat deflection temperature | 90 °C Show Supplier Material materials with Heat deflection temperature of 90 °C | dry | ISO 75-1/-2 | 2 MPa | |
200 °C Show Supplier Material materials with Heat deflection temperature of 200 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Melting point | 295 °C Show Supplier Material materials with Melting point of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Thermal diffusivity | 9.82e-07 mm²/s Show Supplier Material materials with Thermal diffusivity of 9.82e-07 mm²/s | dry | - | ||
Vicat softening temperature | 250 °C Show Supplier Material materials with Vicat softening temperature of 250 °C | dry | ISO 306 | 50°C/h 50N |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 475 V Show Supplier Material materials with Comparative tracking index of 475 V | dry | IEC 60112 | |
Dielectric constant | 3.2 [-] Show Supplier Material materials with Dielectric constant of 3.2 [-] | dry | IEC 62631-2-1 | 1MHz |
3.6 [-] Show Supplier Material materials with Dielectric constant of 3.6 [-] | dry | IEC 62631-2-1 | 100Hz | |
4 [-] Show Supplier Material materials with Dielectric constant of 4 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Dielectric constant of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Dielectric strength | 15 kV/mm Show Supplier Material materials with Dielectric strength of 15 kV/mm | conditioned | IEC 60243-1 | |
25 kV/mm Show Supplier Material materials with Dielectric strength of 25 kV/mm | dry | IEC 60243-1 | ||
Dissipation factor | 120 [-] Show Supplier Material materials with Dissipation factor of 120 [-] | dry | IEC 62631-2-1 | 100Hz |
190 [-] Show Supplier Material materials with Dissipation factor of 190 [-] | dry | IEC 62631-2-1 | 1MHz | |
1000 [-] Show Supplier Material materials with Dissipation factor of 1000 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
6500 [-] Show Supplier Material materials with Dissipation factor of 6500 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Surface resistivity | 1e+13 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+13 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+07 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+07 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 913 g/cm³ Show Supplier Material materials with Density of melt of 913 g/cm³ | dry | - | |
Shrinkage | 2 % Show Supplier Material materials with Shrinkage of 2 % | dry | Sim. to ISO 294-4 | Parallel |
2 % Show Supplier Material materials with Shrinkage of 2 % | dry | Sim. to ISO 294-4 | Normal | |
Specific heat capacity melt | 2550 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2550 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.24 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.24 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Convoluted Tubes, Front End Accessory Drive Parts: Belt Tensioner,Damping bands, Shoes and Bushings |