General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.64 g/cm³ Show Supplier Material materials with Density of 1.64 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.6 % Show Supplier Material materials with Moisture absorption of 1.6 % | dry | Sim. to ISO 62 |
Water absorption | 4.2 % Show Supplier Material materials with Water absorption of 4.2 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Thickness | Testing Standard | Comment |
---|---|---|---|---|---|---|
Elastic modulus | 17.5 GPa Show Supplier Material materials with Elastic modulus of 17.5 GPa | dry | 1 mm | ISO 527-1/-2 | ||
17.5 GPa Show Supplier Material materials with Elastic modulus of 17.5 GPa | dry | 1 mm | ISO 527-1/-2 | |||
18.5 GPa Show Supplier Material materials with Elastic modulus of 18.5 GPa | conditioned | ISO 527-1/-2 | ||||
Elongation | 2.3 % Show Supplier Material materials with Elongation of 2.3 % | conditioned | ISO 527-1/-2 | |||
2.4 % Show Supplier Material materials with Elongation of 2.4 % | dry | 1 mm | ISO 527-1/-2 | |||
2.5 % Show Supplier Material materials with Elongation of 2.5 % | dry | 1 mm | ISO 527-1/-2 | |||
Flexural modulus | 16.5 GPa Show Supplier Material materials with Flexural modulus of 16.5 GPa | dry | ISO 178 | |||
17.5 GPa Show Supplier Material materials with Flexural modulus of 17.5 GPa | conditioned | ISO 178 | ||||
Flexural yield strength | 350 MPa Show Supplier Material materials with Flexural yield strength of 350 MPa | conditioned | ISO 178 | |||
400 MPa Show Supplier Material materials with Flexural yield strength of 400 MPa | dry | ISO 178 | ||||
Impact strength, Charpy notched | 23 °C | 12.5 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 12.5 kJ/m² | conditioned | ISO 179/1eA | ||
23 °C | 14.5 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 14.5 kJ/m² | dry | ISO 179/1eA | |||
Impact strength, Charpy unnotched | 23 °C | 75 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 75 kJ/m² | conditioned | ISO 179/1eU | ||
23 °C | 90 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 90 kJ/m² | dry | ISO 179/1eU | |||
Tensile strength | 240 MPa Show Supplier Material materials with Tensile strength of 240 MPa | conditioned | ISO 527-1/-2 | |||
270 MPa Show Supplier Material materials with Tensile strength of 270 MPa | dry | 1 mm | ISO 527-1/-2 | at low thickness | ||
280 MPa Show Supplier Material materials with Tensile strength of 280 MPa | dry | 1 mm | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 2e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 2e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 5e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Heat deflection temperature | 245 °C Show Supplier Material materials with Heat deflection temperature of 245 °C | dry | ISO 75-1/-2 | 2 MPa | |
Melting point | 315 °C Show Supplier Material materials with Melting point of 315 °C | dry | ISO 11357-1/-3 | 10°C/min |
Electrical
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | Mobile Phone Mid-Frame | |
Certifications | Yellow Card Available | |
Fillers | 50% Glass Fiber |