EcoPaXX® Q170E-H

Want to keep this datasheet? Save it now in your required format

Description

EcoPaXX® is our bio-based, high-performance polyamide (PA410) that offers outstanding performance across the board, while being made mainly from tropical castor beans which don’t compete with the food chain.
EcoPaXX® belongs to the family of long-chain polyamides, which offer exceptional performance in the most demanding of environments. That includes excellent chemical resistance, low moisture absorption, combined with a very high melting point (highest of all bio-plastics) and high crystallization rate (typical for engineering plastics like PA66 and PA46).
EcoPaXX® has the lowest carbon footprint amongst common polyamides. This is because the amount of carbon dioxide emitted during the production of EcoPaXX® is offset by the amount absorbed in plant growth, and in particular by the riccinus communis – the tropical castor bean plant that makes up some 70% of EcoPaXX®. Externally certified lifecycle analysis (LCA) data is available upon request.

Datasheet URL:

EcoPaXX® Q170E-H

This material data has been provided by DSM.

"Typical" values were obtained via a literature search. "Predicted" values were imputed via artificial intelligence technology. While we have placed significant efforts in ensuring data accuracy, "typical" and "predicted" data should be considered indicative and verified by appropriate material testing. Please do contact us if additional information on the the predicted data method is required.
All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionTesting Standard

Bio-based content

70 %

Show Supplier Material materials with Bio-based content of 70 %

dry

ASTM D6866-12 Method B

Density

1.09 g/cm³

Show Supplier Material materials with Density of 1.09 g/cm³

dry

ISO 1183

Moisture absorption

1.9 %

Show Supplier Material materials with Moisture absorption of 1.9 %

dry

Sim. to ISO 62

Water absorption

5.8 %

Show Supplier Material materials with Water absorption of 5.8 %

dry

Sim. to ISO 62

Mechanical

PropertyTemperatureValueConditionTesting Standard

Elastic modulus

1.6 GPa

Show Supplier Material materials with Elastic modulus of 1.6 GPa

conditioned

ISO 527-1/-2

3.2 GPa

Show Supplier Material materials with Elastic modulus of 3.2 GPa

dry

ISO 527-1/-2

120 °C

0.6 GPa

Show Supplier Material materials with Elastic modulus of 0.6 GPa

dry

ISO 527-1/-2

140 °C

0.52 GPa

Show Supplier Material materials with Elastic modulus of 0.52 GPa

dry

ISO 527-1/-2

Elongation

20 %

Show Supplier Material materials with Elongation of 20 %

dry

ISO 527-1/-2

50 %

Show Supplier Material materials with Elongation of 50 %

conditioned

ISO 527-1/-2

120 °C

200 %

Show Supplier Material materials with Elongation of 200 %

dry

ISO 527-1/-2

140 °C

200 %

Show Supplier Material materials with Elongation of 200 %

dry

ISO 527-1/-2

Elongation at yield

4.6 %

Show Supplier Material materials with Elongation at yield of 4.6 %

dry

ISO 527-1/-2

20 %

Show Supplier Material materials with Elongation at yield of 20 %

conditioned

ISO 527-1/-2

Impact strength, Charpy notched

-30 °C

4 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 4 kJ/m²

dry

ISO 179/1eA

-30 °C

4.5 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 4.5 kJ/m²

conditioned

ISO 179/1eA

23 °C

5.5 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 5.5 kJ/m²

dry

ISO 179/1eA

23 °C

12 kJ/m²

Show Supplier Material materials with Impact strength, Charpy notched of 12 kJ/m²

conditioned

ISO 179/1eA

Tensile strength

45 MPa

Show Supplier Material materials with Tensile strength of 45 MPa

conditioned

ISO 527-1/-2

55.0 MPa

Show Supplier Material materials with Tensile strength of 55.0 MPa

dry

ISO 527-1/-2

120 °C

38 MPa

Show Supplier Material materials with Tensile strength of 38 MPa

dry

ISO 527-1/-2

140 °C

32 MPa

Show Supplier Material materials with Tensile strength of 32 MPa

dry

ISO 527-1/-2

Thermal

PropertyValueConditionTesting StandardPressureComment

Heat deflection temperature

75 °C

Show Supplier Material materials with Heat deflection temperature of 75 °C

dry

ISO 75-1/-2

2 MPa

175 °C

Show Supplier Material materials with Heat deflection temperature of 175 °C

dry

ISO 75-1/-2

0.45 MPa

Melting point

250 °C

Show Supplier Material materials with Melting point of 250 °C

dry

ISO 11357-1/-3

10°C/min

Rheological Properties

PropertyTemperatureValueConditionTesting Standard

Melt mass-flow rate

280 °C

24 g/10min

Show Supplier Material materials with Melt mass-flow rate of 24 g/10min

dry

ISO 1133

Melt volume-flow rate

280 °C

26 cm³/10min

Show Supplier Material materials with Melt volume-flow rate of 26 cm³/10min

dry

ISO 1133

Viscosity number

170 cm³/gr

Show Supplier Material materials with Viscosity number of 170 cm³/gr

dry

ISO 307, 1157, 1628

Technological properties