General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.53 g/cm³ Show Supplier Material materials with Density of 1.53 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.8 % Show Supplier Material materials with Moisture absorption of 1.8 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 8 GPa Show Supplier Material materials with Elastic modulus of 8 GPa | conditioned | ISO 527-1/-2 | |
12.5 GPa Show Supplier Material materials with Elastic modulus of 12.5 GPa | dry | ISO 527-1/-2 | ||
Elongation | 1.7 % Show Supplier Material materials with Elongation of 1.7 % | dry | ISO 527-1/-2 | |
2.5 % Show Supplier Material materials with Elongation of 2.5 % | conditioned | ISO 527-1/-2 | ||
Flexural modulus | 8 GPa Show Supplier Material materials with Flexural modulus of 8 GPa | conditioned | ISO 178 | |
12.5 GPa Show Supplier Material materials with Flexural modulus of 12.5 GPa | dry | ISO 178 | ||
Impact strength, Charpy notched | 23 °C | 9 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 9 kJ/m² | dry, conditioned | ISO 179/1eA |
Impact strength, Charpy unnotched | 23 °C | 35 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 35 kJ/m² | dry | ISO 179/1eU |
23 °C | 40 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 40 kJ/m² | conditioned | ISO 179/1eU | |
Tensile strength | 100 MPa Show Supplier Material materials with Tensile strength of 100 MPa | conditioned | ISO 527-1/-2 | |
140 MPa Show Supplier Material materials with Tensile strength of 140 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 3.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 3.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
4.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 4.5e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Flammability | V-0 | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Glass transition temperature | 75 °C Show Supplier Material materials with Glass transition temperature of 75 °C | dry | ISO 11357-1/-2 | 10°C/min | ||
Glow Wire Flammability Index | 960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 3 mm | ||
960 °C Show Supplier Material materials with Glow Wire Flammability Index of 960 °C | dry | IEC 60695-2-12 | 0.75 mm | |||
Glow Wire Ignition Temperature | 960 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 960 °C | dry | IEC 60695-2-13 | 3 mm | ||
960 °C Show Supplier Material materials with Glow Wire Ignition Temperature of 960 °C | dry | IEC 60695-2-13 | 0.75 mm | |||
Heat deflection temperature | 290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 2 MPa | ||
290 °C Show Supplier Material materials with Heat deflection temperature of 290 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 295 °C Show Supplier Material materials with Melting point of 295 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 0.75 mm |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 425 V Show Supplier Material materials with Comparative tracking index of 425 V | dry | IEC 60112 | |
Dielectric constant | 3.9 [-] Show Supplier Material materials with Dielectric constant of 3.9 [-] | dry | IEC 60250 | 1GHz |
4.1 [-] Show Supplier Material materials with Dielectric constant of 4.1 [-] | dry | IEC 62631-2-1 | 1MHz | |
4.2 [-] Show Supplier Material materials with Dielectric constant of 4.2 [-] | conditioned | IEC 60250 | 1GHz | |
4.9 [-] Show Supplier Material materials with Dielectric constant of 4.9 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
Dielectric strength | 31 kV/mm Show Supplier Material materials with Dielectric strength of 31 kV/mm | conditioned | IEC 60243-1 | |
33 kV/mm Show Supplier Material materials with Dielectric strength of 33 kV/mm | dry | IEC 60243-1 | ||
Dissipation factor | 220 [-] Show Supplier Material materials with Dissipation factor of 220 [-] | dry | IEC 60250 | 1GHz |
250 [-] Show Supplier Material materials with Dissipation factor of 250 [-] | dry | IEC 62631-2-1 | 1MHz | |
650 [-] Show Supplier Material materials with Dissipation factor of 650 [-] | conditioned | IEC 60250 | 1GHz | |
700 [-] Show Supplier Material materials with Dissipation factor of 700 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+10 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+10 Ω·cm | conditioned | IEC 62631-3-1 | |
1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 62631-3-1 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Application areas | WtB and BtB Connectors, Arc Chamber | |
Certifications | Yellow Card Available | |
Fillers | 30% Glass Fiber |