General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Bio-based content | 56.0 % Show Supplier Material materials with Bio-based content of 56.0 % | dry | ASTM D6866-12 Method B |
Density | 1.05 g/cm³ Show Supplier Material materials with Density of 1.05 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.7 % Show Supplier Material materials with Moisture absorption of 1.7 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elastic modulus | 0.9 GPa Show Supplier Material materials with Elastic modulus of 0.9 GPa | conditioned | ISO 527-1/-2 | ||
1.8 GPa Show Supplier Material materials with Elastic modulus of 1.8 GPa | dry | ISO 527-1/-2 | |||
120 °C | 0.35 GPa Show Supplier Material materials with Elastic modulus of 0.35 GPa | dry | ISO 527-1/-2 | ||
160 °C | 0.22 GPa Show Supplier Material materials with Elastic modulus of 0.22 GPa | dry | ISO 527-1/-2 | ||
180 °C | 0.17 GPa Show Supplier Material materials with Elastic modulus of 0.17 GPa | dry | ISO 527-1/-2 | ||
200 °C | 0.12 GPa Show Supplier Material materials with Elastic modulus of 0.12 GPa | dry | ISO 527-1/-2 | ||
Elongation | 30 % Show Supplier Material materials with Elongation of 30 % | dry | ISO 527-1/-2 | ||
50 % Show Supplier Material materials with Elongation of 50 % | conditioned | ISO 527-1/-2 | |||
120 °C | 50 % Show Supplier Material materials with Elongation of 50 % | dry | ISO 527-1/-2 | ||
160 °C | 50 % Show Supplier Material materials with Elongation of 50 % | dry | ISO 527-1/-2 | ||
180 °C | 50 % Show Supplier Material materials with Elongation of 50 % | dry | ISO 527-1/-2 | ||
200 °C | 50 % Show Supplier Material materials with Elongation of 50 % | dry | ISO 527-1/-2 | ||
Elongation at yield | 6 % Show Supplier Material materials with Elongation at yield of 6 % | dry | ISO 527-1/-2 | ||
20 % Show Supplier Material materials with Elongation at yield of 20 % | conditioned | ISO 527-1/-2 | |||
Flexural modulus | 0.95 GPa Show Supplier Material materials with Flexural modulus of 0.95 GPa | conditioned | ISO 178 | ||
1.8 GPa Show Supplier Material materials with Flexural modulus of 1.8 GPa | dry | ISO 178 | |||
Flexural yield strength | 40 MPa Show Supplier Material materials with Flexural yield strength of 40 MPa | conditioned | ISO 178 | ||
70 MPa Show Supplier Material materials with Flexural yield strength of 70 MPa | dry | ISO 178 | |||
Hardness, Shore D | 72 [-] Show Supplier Material materials with Hardness, Shore D of 72 [-] | dry | ISO 868 | 15s | |
Impact strength, Charpy notched | -30 °C | 20 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 20 kJ/m² | dry | ISO 179/1eA | |
23 °C | 65 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 65 kJ/m² | dry | ISO 179/1eA | ||
23 °C | 75 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 75 kJ/m² | conditioned | ISO 179/1eA |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 1.2e-06 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.2e-06 1/K | dry | ISO 11359-1/-2 | Normal | |
1.4e-06 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.4e-06 1/K | dry | ISO 11359-1/-2 | Parallel | ||
Heat deflection temperature | 75 °C Show Supplier Material materials with Heat deflection temperature of 75 °C | dry | ISO 75-1/-2 | 2 MPa | |
140 °C Show Supplier Material materials with Heat deflection temperature of 140 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Melting point | 250 °C Show Supplier Material materials with Melting point of 250 °C | dry | ISO 11357-1/-3 | 10°C/min |
Rheological Properties
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Density of melt | 0.9 g/cm³ Show Supplier Material materials with Density of melt of 0.9 g/cm³ | dry | - | ||
Melt volume-flow rate | 290 °C | 11 cm³/10min Show Supplier Material materials with Melt volume-flow rate of 11 cm³/10min | dry | ISO 1133 | |
Shrinkage | 1.8 % Show Supplier Material materials with Shrinkage of 1.8 % | dry | ISO 294-4 | Normal | |
2.8 % Show Supplier Material materials with Shrinkage of 2.8 % | dry | ISO 294-4 | Parallel |
Technological properties
Property | ||
---|---|---|
Application areas | Coolant tubing |