General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.23 g/cm³ Show Supplier Material materials with Density of 1.23 g/cm³ | dry | ISO 1183 |
Moisture absorption | 2.3 % Show Supplier Material materials with Moisture absorption of 2.3 % | dry | Sim. to ISO 62 |
Water absorption | 7.6 % Show Supplier Material materials with Water absorption of 7.6 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 3.5 GPa Show Supplier Material materials with Elastic modulus of 3.5 GPa | conditioned | ISO 527-1/-2 | |
6 GPa Show Supplier Material materials with Elastic modulus of 6 GPa | dry | ISO 527-1/-2 | ||
Elongation | 3 % Show Supplier Material materials with Elongation of 3 % | dry | ISO 527-1/-2 | |
12 % Show Supplier Material materials with Elongation of 12 % | conditioned | ISO 527-1/-2 | ||
Flexural modulus | 5.2 GPa Show Supplier Material materials with Flexural modulus of 5.2 GPa | dry | ISO 178 | |
Flexural yield strength | 170 MPa Show Supplier Material materials with Flexural yield strength of 170 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | -30 °C | 6 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 6 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 7 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 7 kJ/m² | dry | ISO 179/1eA | |
23 °C | 15 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 15 kJ/m² | conditioned | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 40 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 40 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 45 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 45 kJ/m² | dry | ISO 179/1eU | |
23 °C | 80 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 80 kJ/m² | conditioned | ISO 179/1eU | |
Tensile strength | 70 MPa Show Supplier Material materials with Tensile strength of 70 MPa | conditioned | ISO 527-1/-2 | |
125 MPa Show Supplier Material materials with Tensile strength of 125 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Thickness | Pressure | Comment |
---|---|---|---|---|---|---|
Coefficient of thermal expansion | 3e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 3e-07 1/K | dry | ISO 11359-1/-2 | Parallel | ||
8e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 8e-07 1/K | dry | ISO 11359-1/-2 | Normal | |||
Flammability | HB | dry | IEC 60695-11-10 | 1.5 mm | UL recognition :Yes | |
Heat deflection temperature | 195 °C Show Supplier Material materials with Heat deflection temperature of 195 °C | dry | ISO 75-1/-2 | 2 MPa | ||
215 °C Show Supplier Material materials with Heat deflection temperature of 215 °C | dry | ISO 75-1/-2 | 0.45 MPa | |||
Melting point | 220 °C Show Supplier Material materials with Melting point of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | ||
Relative temperature index, electrical | 65 °C Show Supplier Material materials with Relative temperature index, electrical of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical impact | 65 °C Show Supplier Material materials with Relative temperature index, mechanical impact of 65 °C | dry | UL746B | 0.75 mm | ||
Relative temperature index, mechanical strength | 65 °C Show Supplier Material materials with Relative temperature index, mechanical strength of 65 °C | dry | UL746B | 0.75 mm | ||
Thermal diffusivity | 1.03e-07 mm²/s Show Supplier Material materials with Thermal diffusivity of 1.03e-07 mm²/s | dry | - |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 600 V Show Supplier Material materials with Comparative tracking index of 600 V | conditioned | IEC 60112 | |
Dielectric constant | 3.5 [-] Show Supplier Material materials with Dielectric constant of 3.5 [-] | dry | IEC 62631-2-1 | 100Hz |
4.5 [-] Show Supplier Material materials with Dielectric constant of 4.5 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
4.7 [-] Show Supplier Material materials with Dielectric constant of 4.7 [-] | dry | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Dielectric constant of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Dielectric strength | 25 kV/mm Show Supplier Material materials with Dielectric strength of 25 kV/mm | conditioned | IEC 60243-1 | |
35 kV/mm Show Supplier Material materials with Dielectric strength of 35 kV/mm | dry | IEC 60243-1 | ||
Dissipation factor | 55 [-] Show Supplier Material materials with Dissipation factor of 55 [-] | dry | IEC 62631-2-1 | 100Hz |
180 [-] Show Supplier Material materials with Dissipation factor of 180 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Dissipation factor of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
1500 [-] Show Supplier Material materials with Dissipation factor of 1500 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Surface resistivity | 1e+14 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+14 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry, conditioned | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 1030 g/cm³ Show Supplier Material materials with Density of melt of 1030 g/cm³ | dry | - | |
Shrinkage | 0.32 % Show Supplier Material materials with Shrinkage of 0.32 % | dry | ISO 294-4 | Parallel |
0.96 % Show Supplier Material materials with Shrinkage of 0.96 % | dry | ISO 294-4 | Normal | |
Specific heat capacity melt | 2400 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2400 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.26 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.26 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Wheel Chair Rims | |
Certifications | Yellow Card Available | |
Fillers | 15% Glass Fiber |