General
Property | Value | Condition | Testing Standard |
---|---|---|---|
Density | 1.4 g/cm³ Show Supplier Material materials with Density of 1.4 g/cm³ | dry | ISO 1183 |
Moisture absorption | 1.7 % Show Supplier Material materials with Moisture absorption of 1.7 % | dry | Sim. to ISO 62 |
Water absorption | 5.6 % Show Supplier Material materials with Water absorption of 5.6 % | dry | Sim. to ISO 62 |
Mechanical
Property | Temperature | Value | Condition | Testing Standard |
---|---|---|---|---|
Elastic modulus | 7 GPa Show Supplier Material materials with Elastic modulus of 7 GPa | conditioned | ISO 527-1/-2 | |
11 GPa Show Supplier Material materials with Elastic modulus of 11 GPa | dry | ISO 527-1/-2 | ||
100 °C | 4.7 GPa Show Supplier Material materials with Elastic modulus of 4.7 GPa | dry | ISO 527-1/-2 | |
120 °C | 4.3 GPa Show Supplier Material materials with Elastic modulus of 4.3 GPa | dry | ISO 527-1/-2 | |
150 °C | 3.8 GPa Show Supplier Material materials with Elastic modulus of 3.8 GPa | dry | ISO 527-1/-2 | |
160 °C | 3.6 GPa Show Supplier Material materials with Elastic modulus of 3.6 GPa | dry | ISO 527-1/-2 | |
180 °C | 3.2 GPa Show Supplier Material materials with Elastic modulus of 3.2 GPa | dry | ISO 527-1/-2 | |
200 °C | 2.6 GPa Show Supplier Material materials with Elastic modulus of 2.6 GPa | dry | ISO 527-1/-2 | |
Elongation | 3.3 % Show Supplier Material materials with Elongation of 3.3 % | dry | ISO 527-1/-2 | |
6.5 % Show Supplier Material materials with Elongation of 6.5 % | conditioned | ISO 527-1/-2 | ||
120 °C | 9.2 % Show Supplier Material materials with Elongation of 9.2 % | dry | ISO 527-1/-2 | |
150 °C | 8.8 % Show Supplier Material materials with Elongation of 8.8 % | dry | ISO 527-1/-2 | |
160 °C | 8.6 % Show Supplier Material materials with Elongation of 8.6 % | dry | ISO 527-1/-2 | |
180 °C | 8.3 % Show Supplier Material materials with Elongation of 8.3 % | dry | ISO 527-1/-2 | |
200 °C | 8 % Show Supplier Material materials with Elongation of 8 % | dry | ISO 527-1/-2 | |
Flexural modulus | 6.4 GPa Show Supplier Material materials with Flexural modulus of 6.4 GPa | conditioned | ISO 178 | |
10 GPa Show Supplier Material materials with Flexural modulus of 10 GPa | dry | ISO 178 | ||
120 °C | 4.7 GPa Show Supplier Material materials with Flexural modulus of 4.7 GPa | dry | ISO 178 | |
160 °C | 4.0 GPa Show Supplier Material materials with Flexural modulus of 4.0 GPa | dry | ISO 178 | |
Flexural yield strength | 170 MPa Show Supplier Material materials with Flexural yield strength of 170 MPa | conditioned | ISO 178 | |
280 MPa Show Supplier Material materials with Flexural yield strength of 280 MPa | dry | ISO 178 | ||
120 °C | 110 MPa Show Supplier Material materials with Flexural yield strength of 110 MPa | dry | ISO 178 | |
160 °C | 90 MPa Show Supplier Material materials with Flexural yield strength of 90 MPa | dry | ISO 178 | |
Impact strength, Charpy notched | -30 °C | 12 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 12 kJ/m² | dry, conditioned | ISO 179/1eA |
23 °C | 15 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 15 kJ/m² | dry | ISO 179/1eA | |
23 °C | 23 kJ/m² Show Supplier Material materials with Impact strength, Charpy notched of 23 kJ/m² | conditioned | ISO 179/1eA | |
Impact strength, Charpy unnotched | -30 °C | 70 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 70 kJ/m² | dry, conditioned | ISO 179/1eU |
23 °C | 95 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 95 kJ/m² | dry | ISO 179/1eU | |
23 °C | 100 kJ/m² Show Supplier Material materials with Impact strength, Charpy unnotched of 100 kJ/m² | conditioned | ISO 179/1eU | |
Tensile strength | 125 MPa Show Supplier Material materials with Tensile strength of 125 MPa | conditioned | ISO 527-1/-2 | |
185 MPa Show Supplier Material materials with Tensile strength of 185 MPa | dry | ISO 527-1/-2 | ||
100 °C | 95 MPa Show Supplier Material materials with Tensile strength of 95 MPa | dry | ISO 527-1/-2 | |
120 °C | 90 MPa Show Supplier Material materials with Tensile strength of 90 MPa | dry | ISO 527-1/-2 | |
150 °C | 75 MPa Show Supplier Material materials with Tensile strength of 75 MPa | dry | ISO 527-1/-2 | |
160 °C | 70 MPa Show Supplier Material materials with Tensile strength of 70 MPa | dry | ISO 527-1/-2 | |
180 °C | 55.0 MPa Show Supplier Material materials with Tensile strength of 55.0 MPa | dry | ISO 527-1/-2 | |
200 °C | 45 MPa Show Supplier Material materials with Tensile strength of 45 MPa | dry | ISO 527-1/-2 |
Thermal
Property | Value | Condition | Testing Standard | Pressure | Comment |
---|---|---|---|---|---|
Coefficient of thermal expansion | 1.5e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 1.5e-07 1/K | dry | ISO 11359-1/-2 | Parallel | |
6e-07 1/K Show Supplier Material materials with Coefficient of thermal expansion of 6e-07 1/K | dry | ISO 11359-1/-2 | Normal | ||
Heat deflection temperature | 177 °C Show Supplier Material materials with Heat deflection temperature of 177 °C | dry | ISO 75-1/-2 | 8 MPa | |
200 °C Show Supplier Material materials with Heat deflection temperature of 200 °C | dry | ISO 75-1/-2 | 2 MPa | ||
220 °C Show Supplier Material materials with Heat deflection temperature of 220 °C | dry | ISO 75-1/-2 | 0.45 MPa | ||
Melting point | 220 °C Show Supplier Material materials with Melting point of 220 °C | dry | ISO 11357-1/-3 | 10°C/min | |
Thermal diffusivity | 1.02e-07 mm²/s Show Supplier Material materials with Thermal diffusivity of 1.02e-07 mm²/s | dry | - |
Electrical
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Comparative tracking index | 500 V Show Supplier Material materials with Comparative tracking index of 500 V | dry | IEC 60112 | |
Dielectric constant | 3.3 [-] Show Supplier Material materials with Dielectric constant of 3.3 [-] | dry | IEC 62631-2-1 | 1MHz |
3.5 [-] Show Supplier Material materials with Dielectric constant of 3.5 [-] | dry | IEC 62631-2-1 | 100Hz | |
4.4 [-] Show Supplier Material materials with Dielectric constant of 4.4 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
14.0 [-] Show Supplier Material materials with Dielectric constant of 14.0 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Dissipation factor | 50 [-] Show Supplier Material materials with Dissipation factor of 50 [-] | dry | IEC 62631-2-1 | 100Hz |
150 [-] Show Supplier Material materials with Dissipation factor of 150 [-] | dry | IEC 62631-2-1 | 1MHz | |
1200 [-] Show Supplier Material materials with Dissipation factor of 1200 [-] | conditioned | IEC 62631-2-1 | 1MHz | |
3000 [-] Show Supplier Material materials with Dissipation factor of 3000 [-] | conditioned | IEC 62631-2-1 | 100Hz | |
Surface resistivity | 1e+15 Ω/sq Show Supplier Material materials with Surface resistivity of 1e+15 Ω/sq | conditioned | IEC 62631-3-2 | |
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry, conditioned | IEC 62631-3-1 |
Rheological Properties
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Density of melt | 1200 g/cm³ Show Supplier Material materials with Density of melt of 1200 g/cm³ | dry | - | |
Shrinkage | 0.3 % Show Supplier Material materials with Shrinkage of 0.3 % | dry | ISO 294-4 | Parallel |
1 % Show Supplier Material materials with Shrinkage of 1 % | dry | ISO 294-4 | Normal | |
Specific heat capacity melt | 2170 J/(kg·K) Show Supplier Material materials with Specific heat capacity melt of 2170 J/(kg·K) | dry | - | |
Thermal conductivity of melt | 0.27 W/(m·K) Show Supplier Material materials with Thermal conductivity of melt of 0.27 W/(m·K) | dry | - |
Technological properties
Property | ||
---|---|---|
Application areas | Off-road Vehicle Oil Pans and Reservoirs, Transmission Oil Pans, Fans & Shrouds, Thermoplastic Oil Pan, Cylinder head covers, Instrument panels, Sunroof frame | |
Fillers | 35% Glass Fiber |